Animal/plant proteins (gelatin/gluten) composite sponge with adaptive wet mechanics for rapid hemostasis

Research article Full text access Get rights and content Animal/plant proteins (gelatin/gluten) composite sponge with adaptive wet mechanics for rapid hemostasis Author links open overlay panelLi Yu a, Wei Guo a, Yajie Wen a, Runlan Chen a, Ruihao Lin a, Haiqing Liu a b Show more 2026-10-27 科技资讯

1. Introduction

Uncontrolled hemorrhage remains one of the leading causes of trauma-related mortality worldwide and accounts for ~30–40% of preventable prehospital deaths, highlighting the urgent need for efficient and safe hemostatic materials [1], [2]. Among various hemostatic platforms, three-dimensional porous sponges have attracted considerable attention owing to their high porosity, rapid fluid absorption, and ability to provide a microenvironment for the enrichment of blood cells and coagulation factors [3], [4], [5]. In particular, natural protein-based sponges, such as gelatin sponges, have been widely investigated and clinically applied because of their well-documented biocompatibility, biodegradability, and tissue affinity [6], [7], [8]. However, conventional gelatin sponges can undergo substantial softening and deformation upon blood absorption, resulting in compromised wet-state mechanical stability and wound sealing under non-compressible bleeding conditions [7]. In response to these limitations, shape-memory hemostatic sponges have emerged as a promising strategy by enabling rapid structural recovery upon fluid absorption, thereby facilitating adaptive wound filling and physical sealing [9], [10], [11]. Nevertheless, achieving both rapid shape recovery and sufficient wet-state mechanical stability remains challenging, particularly in biocompatible and biodegradable protein-based systems. Therefore, developing natural protein-based hemostatic sponges with adaptive shape recovery and robust wet-state mechanical properties represents a promising approach for effective non-compressible bleeding control [12], [13].

The development of multicomponent biomaterials represents a promising strategy to address the insufficient wet-state stability and mechanical adaptability of conventional gelatin sponges. This approach leverages the complementary functions of different biomacromolecules to achieve synergistic properties unattainable by single components. Recent advances in natural protein-based hemostatic materials have shown that incorporating functional components or constructing hybrid networks can improve the blood absorption, coagulation, and mechanical performance [14]. For example, gelatin-based composite sponges incorporating functional components have been developed to enhance erythrocyte and platelet interactions and accelerate blood coagulation [15], [16], [17]. Collagen- and other natural protein-based sponges have also been explored to improve mechanical recoverability and hemostatic performance [18]. These advances highlight the potential of protein-based multicomponent systems for overcoming the limitations of conventional gelatin sponges [19]. In parallel, plant-derived proteins have garnered growing interest due to their abundance, low cost, biodegradability, and unique molecular architectures. Owing to their richness in hydrophobic amino acid residues and intermolecular interaction sites, plant proteins can confer unique functionalities and improved stability under physiological conditions to biomaterials. However, their direct application is often hindered by poor solubility, aggregation propensity, and intrinsic brittleness [20]. Hybrid protein materials that combine animal- and plant-derived proteins can more effectively exploit the complementary advantages of both components. Animal proteins generally provide excellent gelation capability, good biocompatibility, and favorable tissue affinity, whereas plant proteins contribute unique hydrophobic interactions, molecular chain entanglement, and abundant noncovalent interactions that enhance structural integrity, toughness, and fatigue resistance [21]. Therefore, the rational integration of animal and plant proteins represents a promising strategy to overcome the intrinsic limitations of single-component protein materials and provides new opportunities for developing next-generation protein-based hemostatic biomaterials with improved mechanical robustness, hemostatic efficacy, and biosafety [22].

Among various plant-derived proteins, wheat gluten has emerged as a promising building block for protein-based biomaterials owing to its unique viscoelasticity, biodegradability, and abundant intermolecular interaction sites [23]. Structurally, wheat gluten is primarily composed of gliadin and glutenin, with glutenin consisting of high- and low-molecular-weight subunits interconnected through disulfide bonds to form a hierarchical polymeric network with characteristic loop-and-train-like chain arrangements, endowing the material with remarkable toughness and energy dissipation capability [24]. Building on these unique structural properties, gluten has recently been explored as an active structural component rather than merely a passive filler [25]. For example, glutenin–chitosan three-dimensional porous scaffolds with tunable stiffness and microstructure have been developed for tissue-engineering applications [26]. Disulfide-crosslinked pectin–glutenin hydrogels and wheat gluten-toughened poly (acrylic acid)-based wet tissue adhesive hydrogels have been developed with enhanced reversibility and toughness, as well as improved fatigue resistance and adhesion strength [27], [28], [29]. These advances demonstrate that gluten can actively regulate network mechanics and energy dissipation through molecular interactions and structural reinforcement. However, its poor water solubility and strong aggregation tendency hinder homogeneous integration with hydrophilic biomacromolecules such as gelatin [30], [31], [32]. In addition, the use of conventional cytotoxic crosslinkers, such as glutaraldehyde, raises concerns regarding biomedical applicability. Therefore, developing a mild and biocompatible strategy to improve gluten dispersion and facilitate its cooperative assembly with hydrophilic proteins is highly desirable [33], [34].

In this study, we integrate the animal and plant proteins to develop a new protein-based hemostatic sponge by combining the hydrophilicity and bioactivity of animal-derived gelatin with the hydrophobicity and structural resilience of plant-derived gluten. In this composite, the gelatin network primarily provides rapid fluid absorption, favorable biocompatibility, and a procoagulant microenvironment, whereas gluten forms a flexible energy-dissipating network through chain entanglement, hydrophobic associations, and disulfide bond-mediated interactions, thereby enhancing structural stability, fatigue resistance, and wet-state shape recovery. Based on the regulation of intermolecular interactions, this strategy achieves an integration of structural stability, biological functionality, and mechanical adaptability through the synergistic construction of covalent and noncovalent interaction networks, thereby providing a new design approach for the development of novel protein-based biomaterials that combine rapid hemostatic capability, biocompatibility and biodegradability.

2. Materials and methods

2.1. Materials

Gelatin (Gel, pharmaceutical grade, gel strength ~240 g Bloom) and genipin were purchased from Aladdin, China. Glutathione (GSH) was obtained from Energy Chemical, China. Wheat Gluten (Glu, reagent grade) was supplied by Macklin, China. GS (a commercial gelatin sponge, model FKS-a) was purchased from Guilin Fukang Medical Equipment Co., Ltd. All chemicals were of analytical grade. DI water was prepared in the laboratory.

2.2. Preparation of gluten dispersion

1.0 g of Glu was ground and sieved through a 150-mesh screen to obtain a homogeneous powder. The resulting Glu powder was added portionwise to 10 mL of GSH solution (0.01 g/mL) and magnetically stirred at room temperature for 12 h to ensure interaction between gluten and GSH. The mixture was then subjected to ultrasonication for 30 min to obtain a stable Glu dispersion. Part of the gluten dispersion was freeze-dried for structure analysis.

2.3. Preparation of Gel-Glu composite sponges

Gel-Glu composite sponges were prepared according to the following procedure. A 10 wt% gelatin solution was made at 37 °C. Subsequently, 0, 0.5, 1.0, 1.5, and 2.0 g of gluten dispersions were added to 5.9 g of 0.84 wt% genipin–PBS solution, respectively, followed by respective addition of 4.0, 3.5, 3.0, 2.5, and 2.0 g of the aforementioned gelatin solution. Then, 0.1 g of glycerol was added, yielding a total precursor mass of 10 g for each mixture. Consequently, the total concentration of gluten and gelatin in each mixture was 4 wt%, and the genipin concentration was 0.5 wt% (Table S1). The mixture was continuously stirred at 37 °C to achieve a semi-gel state, which was poured into a mold and allowed to stand at 37 °C for 24 h to complete gelation. The gel was sequentially soaked and washed with PBS and DI water, pre-frozen at −80 °C for 12 h, and then freeze-dried for 48 h to obtain the Gel-Glu composite sponge. According to the ratios of gelatin to gluten in the sponge, the sponge was designated as Gel-Glu-8/0, Gel-Glu-7/1, Gel-Glu-6/2, Gel-Glu-5/3, and Gel-Glu-4/4.

2.4. Structural and morphological characterization

Fourier-transform infrared (FT-IR) spectra of the lyophilized sponges (in KBr pellet form) were recorded on a Fourier-transform infrared spectrometer (Nicolet IS50, Thermo Fisher Scientific, USA). The spectra were collected over the range of 4000–400 cm−1 with 32 scans. The protein secondary structure contents were calculated from the amide I band (1600–1700 cm−1) using PeakFit V4 software. The secondary structures include α-helix (1650–1660 cm−1), β-sheet (1610–1640 cm−1), β-turn (1660–1700 cm−1), and random coil (1640–1650 cm−1). The internal morphology of the Gel-Glu composite sponges was examined by scanning electron microscopy (SEM, Phenomenon LE). Pore diameter and pore wall thickness were manually measured from SEM images using ImageJ software. A total of 90 pores/pore walls were randomly selected and measured for each sponge. The scale bar in each SEM image was used to calibrate the pixel-to-micrometer conversion. Pore size distribution was plotted as a histogram based on the measured data. The cross-sectional morphology and  the corresponding elemental mapping of carbon (C), oxygen (O), nitrogen (N), and sulfur (S) for the lyophilized Gel-Glu-8/0 and Gel-Glu-5/3 sponges  were observed using the SEM equipped with an energy-dispersive spectrometer (EDS). X-ray photoelectron spectroscopy (XPS) was performed on an ESCALAB Xi spectrometer (Thermo Fisher Scientific, USA) with a monochromatic Al Kα X-ray source (E = 1486.6 eV). The zeta potential of the composite sponges was measured using a particle and molecular charge analyzer (Malvern Zetasizer Nano ZS ZEN3600, UK). Water contact angles were determined with a contact angle goniometer (Biolin Theta Flow, Finland).

2.5. Compression test

Before mechanical testing, the dried sponges were fully hydrated by immersion in PBS until reaching equilibrium. Excess surface liquid was gently removed with filter paper, and the samples were immediately subjected to compression testing. The resulting state was defined as the wet state throughout the mechanical characterization. Compression tests were performed at room temperature using a universal testing machine (DR-502B, Dongguan Dongri Instrument Co., Ltd., China) equipped with a 100 N load sensor. Cylindrical composite sponges with a diameter of 10 mm and a height of 10 mm were used for the compression test. During the experiments, a compressive strain of 70% was applied at a compression rate of 20 mm/min. 50 cyclic compression tests were conducted  for each sponge. The compressive modulus (E) was determined by linear fitting of the initial linear segment (0–10% strain range) of the stress–strain curve, and was calculated according to the following equation.where σ and ε are the compressive stress (kPa) and strain, respectively.

The dissipated energy can be determined from the area enclosed by the loading and unloading stress–strain curves. The equation for calculating the dissipated energy (D) is as follows:where ε, δL, and δU represent the cyclic compressive strain, loading curve, and unloading curve, respectively. D denotes the dissipated energy (kJ/m3).

2.6. Shape fixity ratio (Rf)

The original height of the wet sponge was denoted as H1. The sponge was compressed to 70% strain and maintained in the compressed state for 1 min. The water squeezed out from the sponge was then gently removed using filter paper, followed by unloading. After standing for 30 s, the height of the sponge (H2) was measured.

2.7. Water/blood absorption behavior

The dried composite sponges (diameter: 10 mm, height: 10 mm) were weighed (m1) and then immersed in DI water. After complete absorption of water or blood, the sponges were taken out and reweighed (m2). The absorption capacity was calculated according to the following equation:

To investigate the dynamic water uptake behavior, freeze-dried cylindrical sponges (diameter: 10 mm; height: 10 mm) with mass (m0) were gently placed on the surface of DI water in a Petri dish, allowing water to contact the sponge only through its bottom surface. At predetermined time intervals (1, 5, 10, 20, 30, 60, and 120 s), the sponges were removed, and the unbound surface water was carefully removed using filter paper before immediate weighing to obtain the mass at time t (mt). The dynamic water uptake (Qt, g/g) was calculated as follows:

2.8. Water-triggered recovery rate

The sponge was compressed to 20% of its original height and then rapidly immersed in DI water. The recovery process was recorded using a smartphone at 30 fps. The recovery time was defined as the time required for the sponge to recover to 90% of its original height.

2.9. Porosity

Prior to testing, the volume (V) and mass (m1) of each sponge were measured. The sponge was then immersed in ethanol for 2 h. During immersion, the sponge was placed in a vacuum drying chamber to remove the air trapped within the pores, ensuring complete infiltration of ethanol into the porous structure. Subsequently, the sponge was removed, and excess ethanol on the surface was gently wiped off before weighing to obtain the mass (m2). The porosity was calculated according to the following equation:where ρ is the density of ethanol (0.785 g/cm3).

2.10. In vitro blood clotting test

Sponges (10 mm in diameter, 10 mm in height) were pre-warmed at 37 °C for 20 min. Subsequently, 100 μL of fresh rat whole blood was dropped onto the sponge surface and incubated at 37 °C for 10 min. Then, 10 mL of DI water was slowly added. A small amount of the supernatant was taken, and its absorbance at 540 nm was measured using a microplate reader (SpectraMax Plus384) and recorded as As. For the blank control group, 100 μL of rat blood was incubated at 37 °C for 10 min without the addition of sponges, followed by the slow addition of 10 mL DI water. The absorbance of the resulting supernatant at 540 nm was measured in the same manner and recorded as Ab. The blood clotting index (BCI) was calculated according to the following equation:

2.11. Blood cell and platelet adhesion

Sponges (1.0 × 1.0 × 0.5 cm3) were preheated at 37 °C for 10 min prior to testing. Fresh anticoagulated whole blood was diluted tenfold with PBS to obtain a red blood cell (RBC) suspension. Subsequently, 200 μL of the diluted RBC suspension was dropped onto the surface of each sponge and incubated at 37 °C for 1 h to allow sufficient interaction and adhesion between RBCs and the sponges. After incubation, the sponges were gently rinsed three times with PBS to remove the non-adhered RBCs. Thereafter, 2 mL of DI water was added to each sponge and incubated at room temperature for 30 min to completely lyse the adhered RBCs and release hemoglobin. The absorbance of the lysate at 540 nm was measured and recorded as As. As the reference, 200 μL of the RBC suspension was lysed in 2 mL  of DI water, and the absorbance at 540 nm was measured and recorded as Ab. The RBC adhesion ratio was calculated according to the following equation:

For morphological observation, the sponges treated as described above were directly fixed without the addition of DI water. Specifically, the sponges were fixed in 2.5 wt% glutaraldehyde solution at room temperature for 4 h, followed by sequential dehydration in ethanol/PBS solutions with increasing ethanol concentrations (0–100%, at 10% intervals), with each dehydration step lasting 10 min. Subsequently, the sponges were dried in an oven at 37 °C for 48 h, and the adhesion and morphology of blood cells on the sponge surfaces were observed using SEM.

For platelet adhesion analysis, platelet-rich plasma (PRP) was first obtained by centrifuging fresh rat blood at 3000 rpm for 10 min. The preheated sponges were then immersed in the obtained PRP and subjected to the same procedures as described for RBC adhesion. The only modification was that the fixation time in 2.5 wt% glutaraldehyde solution was reduced to 2 h.

2.12. In vivo hemostasis

All animal experiments were performed using male Sprague Dawley (SD) rats (7–8 weeks old, 200–250 g) purchased from the Fujian Laboratory Animal Center. The sex of the animals had no impact on the findings. All procedures were conducted in accordance with protocols approved by the Animal Ethics Committee of Fujian Normal University (Approval No.: IACUC-20240019). A rat liver puncture hemorrhage model was employed to evaluate the in vivo hemostatic performance of the composite sponges. For the Glu group, 35 mg of dry gluten powder (bulk volume approximately matching the cylindrical sponge implants) was directly loaded into a syringe and delivered to the liver puncture wound after injury. All sponges were prepared as cylindrical specimens (3 mm in height, 5 mm in diameter), loaded into syringes, and stored for subsequent use. SD rats were anesthetized with 2% isoflurane in oxygen for induction and 1% isoflurane for maintenance throughout the surgical procedure. Gauze was placed beneath the liver, and a standardized circular penetrating wound (5 mm in diameter) was created to induce hemorrhage. The hemostatic materials were immediately applied to the wound to control bleeding. The blood loss and bleeding time for each group were recorded. Rats in the control group received no hemostatic treatment.

2.13. Hemolysis assay

Sponges were ground into powders, which were dispersed in PBS to prepare suspensions with concentrations of 0.5, 1.0, 2.0, and 4.0 mg/mL. The suspensions were incubated at 37 °C for 10 min. Subsequently, 1 mL of diluted whole blood (Vblood/VPBS = 1/10) was added to an equal volume of each sponge suspension and incubated at 37 °C for 1 h. The mixtures were then centrifuged at 1000 rpm for 5 min, and the absorbance of the supernatant at 540 nm was measured using the microplate reader. Triton X-100 and PBS served as the positive and negative controls, respectively. The hemolysis ratio was calculated as follows:where Ad, An, and Ap are the absorbance values at 540 nm of the supernatant from the sponge group, the negative control, and the positive control, respectively.

2.14. In vitro degradation

Composite sponges (10 mg) were immersed in centrifuge tubes containing 2 mL of lysozyme solution (≥5000 U/mg) and incubated at 37 °C. The lysozyme solution was replaced once daily. For each sponge, four parallel replicates were prepared. At predetermined time points, sponges were removed, rinsed several times with distilled water, freeze-dried, and weighed. The remaining mass ratio was calculated as follows:where m0 and m1 are the masses of the sponge before and after degradation, respectively.

2.15. Cytocompatibility

Composite sponges (5 mm in diameter, 2 mm in height) were sterilized under UV light. Extracts were obtained by incubating the sponges in culture medium at a mass-to-volume ratio of 0.1 g·mL−1 at 37 °C for 24 h. L929 mouse fibroblasts were seeded into 96-well plates at a density of 5000 cells per well (100 μL cell suspension per well) and cultured for 24 h at 37 °C under 5% CO₂ to allow cell attachment. After removing the original medium, 100 μL of fresh medium containing the material extract was added to each well, and the cells were further cultured for 24 h and 48 h.

At the respective time points, cell viability was assessed qualitatively by double-staining with calcein-AM and propidium iodide (PI) and observing under a fluorescence microscope. Quantitative analysis was performed using a Cell Counting Kit-8 (CCK-8) assay. Briefly, 10 μL of CCK-8 solution was added to each well and incubated for 2 h, after which the absorbance at 450 nm was measured using a microplate reader. Cells cultured in fresh complete medium served as the negative control. The cell viability was calculated as follows:where Aₜ, An and Ab represent the absorbance values of the experimental group, negative control group, and blank group, respectively.

2.16. Histocompatibility evaluation

Male C57BL/6 mice (6–8 weeks old) were acclimatized for one week prior to the experiments. After anesthesia with inhaled isoflurane, the dorsal hair of the mice was removed and the skin was disinfected. A transverse incision (~0.5 cm) was created on the dorsal skin, and a subcutaneous pocket was generated by blunt dissection. UV-sterilized sponge were then implanted into the subcutaneous pocket, followed by wound closure using surgical sutures.

At 3, 7, and 14 days post-implantation, mice were sacrificed and full-thickness skin tissues surrounding the implantation sites were harvested. The tissues were fixed in 4% paraformaldehyde for 24 h, rinsed with running water, dehydrated through a graded ethanol series, cleared in xylene, and embedded in paraffin. Subsequently, tissue sections (5 μm thick) were prepared and dried at 60 °C for 30 min.

For histological analysis, the sections were deparaffinized, rehydrated, and stained with hematoxylin and eosin (H&E). Briefly, the sections were stained with hematoxylin for 8 min, differentiated in 1% hydrochloric acid ethanol for 3–5 s, and blued under running water for 10 min. Thereafter, the sections were counterstained with eosin for 2 min, dehydrated through graded ethanol solutions, cleared with xylene, and mounted with neutral resin. Histological images were acquired using an optical microscope. The inflammatory response, tissue architecture integrity, epidermal regeneration, skin appendage regeneration, and the presence of tissue necrosis at the implantation sites were qualitatively evaluated to assess the histocompatibility of the implanted materials.

3. Results and discussion

3.1. Preparation of Gel-Glu composite sponges

Wheat gluten is a complex protein composed of glutenin and gliadin, which are bridged by disulfide bonds (Fig. 1a). Due to the abundance of intra−/inter-molecular disulfide bonds, hydrogen bonds, and hydrophobic interactions, gluten macromolecular chains tend to undergo self-aggregation, resulting in poor dispersibility (Fig. 1b, water). Upon addition of GSH to the dispersion solution, partial disulfide bonds of gluten are cleaved due to reduction, disrupting the highly aggregated gluten network and exposing previously buried hydrophilic units. These structural changes enhanced molecular hydration and suppressed hydrophobicity-driven aggregation, resulting in a more homogeneous gluten dispersion (Fig. 1b, GSH solution) [35]. Meanwhile, the exposed polypeptide chains underwent rearrangement through hydrogen bonding and hydrophobic interactions, leading to alterations in gluten secondary structures. This was confirmed by deconvolution analysis of the amide I region in the FTIR spectra, which revealed decreased contents of α-helix and random coil structures and increased proportions of β-sheet and β-turn structures after GSH treatment (Fig. S1).These findings demonstrate that GSH-mediated reduction not only improves the dispersibility of gluten but also induces molecular rearrangement within the gluten network, providing a basis for constructing gluten-containing composite materials via solution blending. Therefore, GSH treatment can essentially be regarded as a conformational reconstruction process. This structural reorganization not only improves the dispersibility of gluten but also preserves a relatively high degree of structural order, thereby facilitating its homogeneous distribution within the gelatin matrix and the subsequent construction of an integrated network structure [36].

Fig. 1
  1. Download: Download high-res image (478KB)
  2. Download: Download full-size image

Fig. 1. Schematic illustration of the structural organization, dispersion regulation, and formation mechanism of Gel-Glu composite sponges. (a) Schematic representation of the molecular composition of wheat gluten, which consists of glutenin and gliadin. (b) Photographs showing the dispersion behavior of gluten in water before and after GSH treatment. (c) Schematic illustration of the fabrication process of Gel-Glu composite sponges.

Based on this strategy, Gel-Glu composite sponges were fabricated using GSH-pretreated gluten dispersions (Fig. 1c). Gelatin solution was mixed with the pretreated gluten dispersion, followed by the addition of glycerol as a plasticizer and genipin as a crosslinker. Sponges were subsequently constructed through molding and freeze-drying processes. Five composite sponges containing different gluten contents (0, 0.5, 1.0, 1.5, and 2.0 wt%) were prepared (Fig. S2). During the crosslinking process, genipin reacted with the amino groups present in both gelatin and gluten molecules, forming a stable covalently crosslinked network (Fig. S3). In addition, multiple non-covalent interactions coexisted within the composite, including intermolecular hydrogen bonding, hydrophobic interactions, and residual disulfide bonds.

3.2. Morphology and water-response behavior of Gel-Glu composite sponges

Based on the deformation–recovery behavior, the composite sponges were categorized into a rapid recovery (RR) group, including Gel-Glu-8/0, Gel-Glu-7/1, and Gel-Glu-6/2, and a shape fixing (SF) group, including Gel-Glu-5/3 and Gel-Glu-4/4. The RR group recovered to its original shape immediately after unloading, whereas the SF group temporarily retained the compressed state, but underwent pronounced water-triggered shape recovery upon rehydration (Fig. 2a). This transition should be related to the change of the internal network structure of the composite sponges with increasing gluten content. SEM observations revealed a progressive evolution of the internal pore architecture with increasing gluten content (Fig. 2b). The RR group sponges (Gel-Glu-8/0, Gel-Glu-7/1, and Gel-Glu-6/2) possessed relatively thick pore walls and less interconnected porous structures. In contrast, the SF group composites (Gel-Glu-5/3 and Gel-Glu-4/4) developed a more open and highly interconnected porous network with a more homogeneous cellular morphology. Such a porous architecture is suitable for reversible deformation and elastic energy storage during compression, while facilitating capillary-driven liquid transport through interconnected pathways. The pore size distribution gradually shifted toward smaller diameters with increasing gluten content, suggesting a progressive refinement of the porous architecture (Fig. 2c). Quantitative analysis further confirmed a concomitant decrease in both the average pore diameter and wall thickness (Fig. 2d). These results corroborate that gluten incorporation refined the porous architecture during freeze-drying, resulting in smaller pores, thinner pore walls, and a more interconnected network. Such structural changes are beneficial for capillary-driven liquid transport and reversible deformation. SEM–EDS elemental mapping further verified that all elements were uniformly distributed throughout the composite sponge skeleton, corroborating a good compatibility between gelatin and gluten and the formation of a homogeneous and stable composite network (Fig. S4).

Fig. 2
  1. Download: Download high-res image (729KB)
  2. Download: Download full-size image

Fig. 2. Structural evolution and deformation–recovery mechanisms of Gel-Glu composite sponges. (a) Photographs showing the compression and water-triggered shape recovery behaviors of the rapid recovery (RR) and shape fixing (SF) groups. (b) SEM images of the composite sponges. (c) Pore size distribution of the composite sponges. (d) Quantitative analysis of average pore size and pore wall thickness. (e) Schematic illustration of the compression deformation mechanism of the RR group and the compression-induced shape fixing and water-triggered recovery mechanisms of the SF group.

Based on the above structural characteristics, distinct deformation–recovery mechanisms were proposed for the RR and SF group sponges (Fig. 2e). For the RR group sponges, the relatively dense pore architecture and high network rigidity led to pronounced pore wall buckling, interfacial friction, and local collapse during compression, resulting in substantial irreversible mechanical energy dissipation. Consequently, only a limited amount of elastic energy can be stored in the network, making it difficult to stabilize the compressed state. Upon unloading, the stored elastic energy was rapidly released, allowing the sponges to quickly recover to their original shape. In contrast, the SF group sponges developed significantly stronger gluten-mediated intermolecular interactions, leading to the formation of abundant reversible physical crosslinks, including chain entanglements, hydrophobic associations, hydrogen bonding, and dynamic disulfide bonds. Moreover, the open and highly interconnected porous architecture effectively alleviates irreversible structural damage during compression, enabling a larger proportion of the applied mechanical energy to be stored as elastic energy in the network. As a result, the compressed temporary state could be maintained after unloading. Upon rehydration, the infiltration of water molecules plasticizes the polymer network, increases chain mobility, and facilitates network relaxation and molecular rearrangement. This process triggers the release of the stored elastic energy and ultimately drives the recovery of the sponge to its original configuration [37]. Therefore, with increasing gluten content, the deformation response of the composite sponges gradually evolved from an energy dissipation-dominated mechanism to an energy storage-dominated mechanism, endowing the sponges with pronounced shape-fixing capability and water-triggered shape recovery behavior [9].

Together, increasing the gluten content markedly alters both the pore architecture and intermolecular interactions within the composite sponges. An open and highly interconnected porous network is progressively established, accompanied by strengthened reversible interactions, including chain entanglements, hydrogen bonding, hydrophobic associations, and disulfide bonding. Consequently, the deformation behavior of the sponges gradually evolved from rapid elastic recovery to a shape-fixing mode capable of maintaining a temporary shape and exhibiting water-triggered recovery. These findings indicate that the shape-memory characteristics of the composite sponges can be effectively tailored by regulating the gelatin/gluten ratio to modulate the balance between energy dissipation and energy storage in the network. Moreover, the highly interconnected porous structure, together with the water-responsive recovery behavior, is expected to facilitate rapid liquid transport and absorption, thus providing a favorable structural basis for efficient hemostasis.

3.3. Structural characterization and analysis of the physicochemical properties of Gel-Glu composite sponges

To elucidate the influence of gluten incorporation on the network architecture, mechanical adaptability, and hemostasis-related properties of the composite sponges, their chemical composition, wet-state mechanical properties, surface characteristics, and liquid management capability were systematically characterized. FTIR spectra revealed the characteristic protein amide absorption bands including amide I (~1650 cm−1), amide II (~1540 cm−1), and amide III (~1240 cm−1) (Fig. S5). Quantitative analysis of the secondary structure based on Gaussian deconvolution of the amide I region (1600–1700 cm−1) demonstrated that the incorporation of gluten induced substantial conformational reconstruction in the composite network (Fig. S6). The neat gelatin sponge (Gel-Glu-8/0) contained a predominant β-turn content (63.86%) with no detectable α-helical component, consistent with the disrupted triple-helical structure of gelatin after collagen hydrolysis. Upon gluten incorporation (Gel-Glu-5/3), the α-helix content increased from 0 to 15.74%, whereas the β-turn content decreased from 63.86% to 48.76%; meanwhile, the random coil content increased slightly from 12.41% to 14.05% and the β-sheet content reduced marginally from 23.74% to 21.46%. These changes suggest that gluten incorporation induced protein conformational rearrangement through hydrogen bonding, hydrophobic interactions, and genipin-mediated crosslinking, and establishing a molecular structural basis for improving mechanical properties and liquid management behavior. The high-resolution C 1 s spectra of Gel-Glu-8/0 and Gel-Glu-5/3 (Fig. S7) were deconvoluted into three components corresponding to C–C/C–H, C–N/C–O, and O=C–N/C=O groups. Compared with the Gel-Glu-8/0, the C–N/C–O component shifted from 286.27 to 285.96 eV, while the high-binding-energy carbonyl component shifted from 287.99 to 289.20 eV. These shifts indicate that gluten incorporation altered the electronic environments of nitrogen- and oxygen-containing functional groups, suggesting enhanced intermolecular interactions between gelatin and gluten.

The wet-state mechanical properties of the sponges were subsequently evaluated by cyclic compression tests. Upon hydration, the commercial gelatin sponge (GS) rapidly softened and generated a compressive stress of less than 1.0 kPa at 70% strain throughout cyclic compression (Fig. S8), indicating its inability to maintain wound compression under repeated loading. The Gel-Glu composite sponges, however, maintained stable mechanical responses throughout cyclic compression (Fig. 3a). Surprisingly, Gel-Glu-8/0 fractured during the first loading cycle (Fig. S9), whereas all gluten-containing composite sponges remained structurally intact throughout cyclic compression, substantiating that gluten incorporation markedly improved the structural integrity of the sponges under repeated compression. Especially, the loading–unloading curves of Gel-Glu-5/3 and Gel-Glu-4/4 showed a high degree of overlap for 50 cycles, substantiating that gluten incorporation significantly enhanced the structural durability of the sponges under loading-unloading cycles. As the gluten content increased, the compressive strength of the sponges gradually decreased from ~27 kPa for Gel-Glu-8/0 to 15 kPa for Gel-Glu-4/4 (Fig. 3b), reflecting a transition from a rigid network to a more deformable architecture with greater deformation recoverability. All composite sponges nevertheless exhibited substantially higher wet compressive strength than GS, attesting to greater resistance to structural collapse under wet conditions. Meanwhile, the shape fixity ratio increased markedly from ~3% and 5% for Gel-Glu-7/1 and Gel-Glu-6/2 to ~65% and 68% for Gel-Glu-5/3 and Gel-Glu-4/4, respectively. Notably, while maintaining high shape fixity, both Gel-Glu-5/3 and Gel-Glu-4/4 rapidly recovered their original shape within 5 s upon contact with water (Video S1, Video S2), evidencing an optimal combination of shape fixation and rapid water-triggered shape recovery. Such high shape fixity enables the compressed sponges to be readily implanted into irregular or deep wounds, while their rapid expansion upon contact with blood or tissue fluid allows them to exert sustained mechanical support and tamponade at the wound site. Among all formulations, Gel-Glu-5/3 achieved a balance between structural support and shape adaptability, with a compressive strength of ~20 kPa together with a shape fixity ratio of nearly 70%.

The cyclic energy dissipation results further revealed the evolution of the mechanical response of the sponge network (Fig. 3c). Gel-Glu-7/1 showed relatively high energy dissipation during cyclic compression, noting that a large proportion of the applied mechanical energy was irreversibly dissipated through pore wall friction, buckling, and local collapse. In contrast, Gel-Glu-5/3 showed significantly lower energy dissipation and maintained a relatively stable hysteresis loop area throughout the compression cycles, suggesting reduced structural damage and more efficient elastic energy storage. This behavior can be attributed to the combined effects of the refined porous architecture and the progressively strengthened reversible intermolecular interactions with increasing gluten content, including chain entanglement, hydrophobic association, hydrogen bonding, and dynamic disulfide bonds. These reversible interactions synergistically dissipate mechanical stress while storing elastic energy during deformation, thereby imparting enhanced fatigue resistance and shape-fixation capability. Together, these results demonstrate that gluten incorporation fundamentally altered the mechanical response of the sponge, shifting it from a structure dominated by irreversible energy dissipation to one capable of simultaneously dissipating and storing mechanical energy.

Fig. 3
  1. Download: Download high-res image (558KB)
  2. Download: Download full-size image

Fig. 3. (a) Cyclic compression stress–strain curves of wet Gel-Glu composite sponges over 50 loading–unloading cycles. (b) Compressive strength at 70% compressive strain and shape fixity ratio of the composite sponges. (c) Evolution of energy dissipation during cyclic compression for Gel-Glu-7/1 and Gel-Glu-5/3. (d) Compressive modulus and porosity of the composite sponges. (e) Dynamic liquid absorption behavior of the composite sponges. (f) Water absorption capacity and blood absorption capacity of the composite sponges. (g) Zeta potential of the composite sponges. Data are presented as mean ± SD (n = 3 independent samples). *p < 0.05, **p < 0.01, ***p < 0.001.

As the gluten content increased, the compressive modulus gradually decreased from ~27 kPa for Gel-Glu-8/0 to ~5 kPa for Gel-Glu-4/4 (Fig. 3d), confirming that gluten incorporation reduced the overall stiffness of the sponge. Notably, Gel-Glu-5/3 had a compressive modulus of 6.31 kPa, which falls within the reported stiffness range of native soft tissues [38], including liver (4.0–6.5 kPa) [39], adipose tissue (1.6–5.5 kPa) [40], and kidney (4.0–8.0 kPa) [41]. This moderate stiffness may help reduce mechanical mismatch with surrounding soft tissues while preserving sufficient compliance for wound filling. By comparison, the higher modulus of Gel-Glu-8/0 may increase the mechanical mismatch with relatively compliant tissues such as liver and adipose tissue. In addition, the porosity increased from ~40% to ~70% with increasing gluten content (Fig. 3d). Strikingly, this increase occurred despite the progressive reduction in pore diameter (Fig. 2d), suggesting that gluten regulated the formation of a more refined porous architecture consisting of a larger number of interconnected micropores separated by thinner pore walls, rather than fewer large pores. Such a highly porous yet fine cellular structure facilitated rapid fluid transport while reducing irreversible pore-wall collapse during compression and contributing to the superior shape-fixing and water-triggered shape recovery behaviors.

Benefiting from the optimized pore architecture, the composite sponges displayed rapid liquid absorption kinetics (Fig. 3e). In particular, the faster liquid uptake of sponges with higher gluten contents stemmed from their more open and highly interconnected porous structures, which facilitated rapid liquid infiltration and distribution throughout the sponge. Accordingly, both the water absorption capacity and blood absorption capacity increased significantly with increasing gluten content (Fig. 3f), i.e., Gel-Glu-5/3 and Gel-Glu-4/4 reached water absorption capacities of ~13 g·g−1 and blood absorption capacities ~12 g·g−1, both of which were substantially higher than those of Gel-Glu-8/0. Gluten incorporation also markedly altered the surface properties of the sponges. Zeta potential gradually increased with increasing gluten content, corresponding to a reduction in the surface negative charge density (Fig. 3g). This change is expected to weaken the electrostatic repulsion between the sponge surface and negatively charged blood cells, thereby facilitating the adhesion and accumulation of erythrocytes and platelets.

Together, gluten incorporation transformed the internal sponge network from a conventional rigid, energy-dissipative structure into a more compliant network capable of both energy dissipation and elastic energy storage. Consequently, the composite sponges exhibited markedly enhanced shape-fixation capability, fatigue resistance, capillary-driven liquid transport, and liquid management performance while maintaining sufficient mechanical strength. Among all formulations, Gel-Glu-5/3 achieved the optimal balance between structural stability and functional adaptability.

3.4. In vitro hemostatic performance of Gel-Glu composite sponges

To evaluate the in vitro hemostatic performance of the composite sponges, their blood coagulation behavior, erythrocyte adhesion, and platelet activation were investigated. In the in vitro blood clotting test (Fig. 4a), deep red solutions surrounded  the commercial gelatin sponge (GS) because a considerable amount of blood was not clotted by GS, whereas much lighter red solutions surrounded  the Gel-Glu composite sponges, indicating their more rapid blood coagulation. The amount of non-clotted blood decreased with increasing gluten content, suggesting that gluten incorporation accelerated the coagulation process. Notably, both Gel-Glu-5/3 and Gel-Glu-4/4 achieved complete blood coagulation within 4 min. The gluten-only (Glu) sample also showed a certain degree of procoagulant activity, which is associated with the intrinsic hemostatic property of gluten, its ability to enrich blood cells during liquid absorption, and the local concentration of blood cells achieved during liquid absorption. However, in the absence of a stable three-dimensional porous architecture, its coagulation performance was inferior to that of the composite sponges, highlighting the synergistic contribution of the gelatin framework and gluten network to efficient hemostasis. The blood clotting index (BCI) results quantitatively supported these observations (Fig. 4b). Compared with GS and Gel-Glu-8/0, all composite sponges showed lower BCI values, reflecting more efficient blood coagulation and fewer free erythrocytes in the supernatant. The BCI decreased with increasing Glu content in the composite sponges. Among them, Gel-Glu-5/3 and Gel-Glu-4/4 achieved the lowest BCI values of ~16.4% and ~ 15.8%, respectively, confirming their greater blood coagulation ability in vitro.

Fig. 4
  1. Download: Download high-res image (868KB)
  2. Download: Download full-size image

Fig. 4. In vitro hemostatic performance of the Gel-Glu composite sponges. (a) Whole blood coagulation photographs of Glu, GS, and the Gel-Glu composite sponges. (b) BCI. (c) Erythrocyte adhesion ratio. (d) SEM images of adherent erythrocytes (red arrows). (e) SEM images of platelet adhesion (blue arrows) and pseudopodia extensions (white arrows). Data are presented as mean ± SD (n = 3 independent samples). *p < 0.05, **p < 0.01, ***p < 0.001. (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.)

The erythrocyte and platelet adhesion assays further elucidated the mechanism underlying the improved blood coagulation performance of the composite sponges. The erythrocyte capture ratio gradually increased with increasing gluten content (Fig. 4c), rising from ~40% for Gel-Glu-8/0 to ~68% for Gel-Glu-4/4 and substantially exceeding that of the commercial GS sponge (~15%). SEM observations further supported these results (Fig. 4d,e). Only a few sparsely distributed erythrocytes and platelets were observed on the surfaces of GS and Gel-Glu-8/0. In contrast, the gluten-containing composite sponges showed abundant erythrocyte aggregation together with pronounced platelet spreading, pseudopodia extension, and aggregation. In particular, Gel-Glu-5/3 and Gel-Glu-4/4 showed dense erythrocyte coverage accompanied by numerous highly activated platelets, implying enhanced erythrocyte recruitment and platelet activation.

These observations can be attributed to the combined effects of surface charge regulation and structural optimization following gluten incorporation. First, the gradual increase in zeta potential reduced the surface negative charge density, thereby weakening the electrostatic repulsion toward negatively charged erythrocytes and platelets. Second, the higher porosity and more open, interconnected pore architecture facilitated rapid plasma infiltration and the local enrichment of blood cells within the porous network through capillary-driven liquid transport (Fig. 3d–f). The increased local concentration of blood cells further promoted cell–cell interactions and thrombus formation. Collectively, these structural and physicochemical characteristics synergistically enhanced erythrocyte recruitment and platelet-mediated coagulation, thereby accelerating thrombus formation and improving the overall blood coagulation performance of the composite sponges. Among all formulations, Gel-Glu-5/3 achieved coagulation activity comparable to that of Gel-Glu-4/4 while maintaining better wet mechanical performance and fatigue resistance.

3.5. In vivo hemostatic performance of the Gel-Glu composite sponges

To further evaluate the practical hemostatic efficacy of the composite sponges, an in vivo rat liver puncture model was established (Fig. 5a). Owing to its rich vascularization and rapid bleeding, the liver is widely used to assess the hemostatic performance of biomaterials under severe hemorrhagic conditions. After creating a standardized liver puncture wound, different sponges were immediately applied to the bleeding site, and the hemostatic process and hemostatic time were recorded (Fig. 5b). The representative dynamic hemostatic process was recorded by video (Video S3, Video S4, Video S5, Video S6, Video S7, Video S8, Video S9, Video S10). Continuous bleeding was observed throughout the entire observation period in the untreated group, with a large amount of blood surrounding the wound and no formation of stable blood clot. GS partially reduced the bleeding; however, its rapid softening after liquid absorption limited its ability to effectively fill the wound and exert sustained compression on the wound, resulting in obvious blood oozing around the injury site. Similarly, Gel-Glu-8/0, which consisted solely of a gelatin network, failed to prevent bleeding under dynamic physiological conditions, with hemorrhage occurring around the wound within approximately 60 s. In contrast, the Glu group, in which dry gluten powder was directly delivered to the liver puncture wound, promoted local blood aggregation and initial clot formation, supporting the intrinsic procoagulant activity of gluten. Nevertheless, because gluten powder lacks an intact three-dimensional porous sponge structure, it cannot rapidly absorb blood, expand, or effectively fill the wound after contact with blood, making it difficult to establish a stable physical barrier and leading to persistent blood leakage. These results suggest that procoagulant activity alone is insufficient for rapid hemostasis, and effective wound sealing is equally essential.

In comparison, all Gel-Glu composite sponges provided improved hemostatic efficacy. Their interconnected porous architecture enabled rapid blood absorption and the local concentration of blood cells and coagulation factors, while the shape-recovery of the sponges after blood uptake allowed effective wound filling and the provision of both physical tamponade and biological coagulation promotion. As the gluten content increased, the amount of residual blood surrounding the wound gradually decreased, accompanied by a marked reduction in the bleeding area. Significantly, Gel-Glu-5/3 and Gel-Glu-4/4 rapidly formed a stable wound-covering layer with almost no visible blood leakage around the injury site, demonstrating the most effective hemostatic performance.

Fig. 5
  1. Download: Download high-res image (814KB)
  2. Download: Download full-size image

Fig. 5. In vivo hemostatic performance of the Gel-Glu composite sponges. (a) Schematic illustration of the rat liver puncture bleeding model and the hemostatic treatment procedure. Created with BioGDP.com. [44] (b) Representative images of the hemostatic process at 0, 30, 60, 120, and 180 s after sponge application. (c) Blood loss of different experimental groups. (d) Schematic illustration of the hemostatic mechanism of Gel-Glu-5/3. Created with BioGDP.com. [44] Data are presented as mean ± SD (n = 3 independent samples). *p < 0.05, **p < 0.01, ***p < 0.001.

The blood loss measurements further confirmed the above observations (Fig. 5c). Blood loss was greatest in the untreated group (502 ± 34 mg), followed by GS (309 ± 6 mg). All Gel-Glu composite sponges significantly reduced blood loss. Among them, Gel-Glu-5/3 achieved the lowest blood loss (51 ± 4 mg), representing reductions of 83.5% and 50.0% compared with GS and Gel-Glu-8/0, respectively. Gel-Glu-4/4 showed a comparable blood loss (55 ± 3 mg) with no significant difference from Gel-Glu-5/3.

Combined with the in vitro findings, the better in vivo hemostatic performance of Gel-Glu-5/3 can be attributed to the synergistic integration of rapid blood absorption, shape-adaptive wound filling, and coagulation promotion (Fig. 5d). After injection into the irregular wound, the sponge quickly absorbs blood through its interconnected pores, concentrating erythrocytes, platelets, and coagulation factors while swelling to fit the wound geometry for effective tamponade. Mechanistically, the extrinsic and intrinsic pathways converge on Factor X activation, leading to thrombin generation and fibrinogen-to-fibrin conversion, which stabilizes the clot. Platelets are integrated into this cascade rather than acting independently: platelet adhesion, activation, and aggregation form a primary platelet plug that also amplifies thrombin generation and fibrin formation [42], [43]. This is consistent with the observed platelet activation and erythrocyte adhesion (Fig. 4e), as well as the reduced BCI and blood loss, while the underlying molecular coagulation events are not directly characterized in the present study. In parallel, the rapid water-triggered shape recovery and favorable wet-state mechanical properties of Gel–Glu-5/3 enable the sponge to adapt to the wound geometry and maintain physical filling and sealing during clot formation. Collectively, these biological and physical effects contribute to the rapid and stable hemostatic performance of the Gel–Glu-5/3 sponge.

3.6. Biocompatibility and degradation of the Gel-Glu composite sponges

The biocompatibility of the composite sponges was evaluated through cytocompatibility, hemocompatibility, and biodegradation studies. Live/dead staining (Fig. 6a) and CCK-8 assays (Fig. 6b) demonstrated that extracts from all composite sponges caused negligible cytotoxicity after 24 and 48 h of incubation, with cell viabilities consistently exceeding 95% and showing no significant difference from the control group, substantiating satisfactory cytocompatibility. The hemolysis assay (Fig. 6c,d) further confirmed their good hemocompatibility. Compared with the PBS group (negative control), the Triton X-100 group (positive control) showed obvious hemolysis, whereas the supernatants of all composite sponge extracts remained transparent with a faint yellow appearance, similar to that of the PBS group. According to the international standard, a hemolysis ratio below 5% is considered acceptable for hemostatic biomaterials. All Gel-Glu composite sponges maintained hemolysis ratios below 5%, confirming acceptable blood compatibility and providing a solid safety basis for their application as hemostatic materials.

Fig. 6
  1. Download: Download high-res image (2MB)
  2. Download: Download full-size image

Fig. 6. Biocompatibility and degradation performance of the Gel-Glu composite sponges. (a) Representative fluorescence images of live/dead staining of L929 cells after incubation with the composite sponges for 24 and 48 h (green: live cells; red: dead cells). (b) Cell viability of L929 cells cultured with sponge extracts determined by the CCK-8 assay. (c) Hemolysis ratios of the composite sponge extracts. (d) Representative photographs of hemolysis in composite sponge dispersions at different concentrations, PBS (pH 7.4, negative control), and Triton X-100 (positive control). (e) In vitro degradation profiles of the composite sponges in PBS. (f) In vitro degradation profiles of the composite sponges in lysozyme/PBS solution. (g) Representative H&E-stained histological images of wound tissues treated with Gel-Glu-5/3 at 3, 7, and 14 days post-operation. Data are presented as mean ± SD (n = 3 independent samples). (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.)

In vitro biodegradation studies revealed that the composite sponges underwent controllable degradation behavior in both PBS (Fig. 6e) and lysozyme/PBS (Fig. 6f). In PBS, Gel-Glu-8/0 showed the slowest degradation, with degradation ratios of 40.5%, 55.5%, and 100% after 1, 7, and 28 days, respectively. As the gluten content increased, the degradation rate gradually accelerated, and Gel-Glu-4/4 degraded the fastest, reaching complete degradation within 7 days. Throughout the degradation process, the sponges mainly underwent swelling, softening, and eventual disintegration. In the lysozyme/PBS medium, degradation was further accelerated, with degradation ratios ranging from 44% to 75% after 7 days, and all sponges were almost completely degraded within 14 days, accompanied by pronounced fragmentation (Fig. S10). This accelerated degradation is mainly attributed to lysozyme infiltration into the porous network, which induces progressive structural erosion from the surface to the interior, weakens intermolecular non-covalent interactions, and ultimately disrupts the sponge framework. Consequently, the degradation mode shifted from “swelling–dissolution” in PBS to “erosion–fragmentation” in the presence of lysozyme [45]. Furthermore, the open and interconnected pore architecture facilitated liquid penetration and bulk hydration, thereby further accelerating the degradation process [46], [47]. Overall, modulation of the gluten content enabled simultaneous regulation of the network composition and pore architecture, allowing the degradation behavior of the composite sponges to be tailored to meet different clinical requirements for material residence time.

To evaluate the in vivo tissue compatibility of Gel-Glu-5/3, histological analysis of the implantation site was performed using H&E staining (Fig. 6g). The H&E staining results showed that in the three groups of mice with sponge subcutaneous implantation at 3 days, 7 days, and 14 days, no epidermal rupture, tissue necrosis, or large-scale abscess formation was observed in the skin tissues; the subcutaneous muscle layer structure was intact, and the muscle fibers showed no degenerative damage; there were no large amounts of inflammatory cells penetrating the fascia and infiltrating the muscle tissue. At 3 days of implantation, only a few scattered inflammatory cells were present at the material-tissue interface, and almost no new blood vessels were formed; in the 7-day group, the degree of inflammatory infiltration was moderate, and a small number of microvessels began to form; in the 14-day group, a large number of new microvessels could be seen in the interface and the pore of the scaffold, while the surrounding tissue architecture remained intact.

Despite the promising hemostatic performance, several limitations should be acknowledged. The antibacterial properties and tissue adhesion of the Gel–Glu sponge were not systematically investigated, which may limit its application in infected or highly exudative wounds. In addition, the molecular mechanisms underlying platelet activation and coagulation were not directly characterized. Future studies should further evaluate antibacterial activity, tissue adhesion, and coagulation-related molecular mechanisms to broaden the potential applications of Gel–Glu sponges.

4. Conclusions

In this study, gelatin–gluten composite sponges with tunable network structures were successfully developed by regulating the gluten content, and the relationships among network architecture, wet-state mechanical properties, and hemostatic performance were elucidated. Gluten incorporation transformed the sponge network from an energy-dissipation-dominated structure to an adaptive structure capable of both energy dissipation and elastic energy storage, endowing the composites with enhanced fatigue resistance, shape-fixing ability, and wet-state structural stability. In particular, Gel-Glu-5/3 achieved a balanced combination of a compressive modulus of 6.31 kPa, a shape fixity ratio of ~65%, and rapid water-triggered shape recovery within 5 s, while maintaining a high blood absorption capacity (>12 g·g−1). Benefiting from its interconnected porous structure, optimized surface charge, and favorable mechanical properties, Gel-Glu-5/3 effectively promoted erythrocyte adhesion, platelet activation, and blood clot formation, resulting in the lowest blood loss (51 ± 4 mg) in the rat liver injury model while maintaining good cytocompatibility, hemocompatibility, and biodegradability. These findings demonstrate that integrating animal- and plant-derived proteins provides an effective strategy for designing high-performance hemostatic sponges and offers promising potential for rapid hemorrhage control.

CRediT authorship contribution statement

Li Yu: Writing – original draft, Methodology, Data curation. Wei Guo: Writing – review & editing. Yajie Wen: Writing – review & editing. Runlan Chen: Writing – review & editing. Ruihao Lin: Writing – review & editing. Haiqing Liu: Writing – review & editing, Supervision, Resources, Project administration, Funding acquisition.

来源 查看原文

版权申明 本网站立足国家海洋药物和生物制品产业联盟,致力于打造海洋生物医药“产学研用”一站式、综合性资讯共享服务平台,促进我国海洋药物和功能制品“资源链、科技链、产业链、应用链”协同创新、深度融合发展。本文转载自原文来源。版权归原作者及原来出处所有,部分文章未能联系到原作者,在此深表歉意。如涉及版权问题,请留言联系我们协商处理(邮箱:czhang@tio.org.cn),侵权内容将即刻删除。

免责声明 本文仅代表作者个人观点,与本平台立场无关。本站不对内容真实性、完整性、时效性作保证,仅供参考,请读者自行核实。