Research article Full text access Get rights and content Mitochondrial-mediated apoptosis induced by CS-(HMA-co-DEAEMA) hydrogel: A chitosan-based biomaterial exhibiting selective cytotoxicity toward HT-29 and HEK-293 cancer cells Author links open overlay panelAshlesha P. Kawale a, Anand Patel b, Shiwani Singh c, Paramjeet Yadav c, Nishant Shekhar a c, Arti Srivastava a , Arbind Acharya b , Rajesh Kumar c , Neha Jain d Show more 2026-10-30 科技资讯

Abstract

Colorectal cancer remains a critical therapeutic challenge, requiring the development of biocompatible and efficient treatment systems. In this study, chitosan-based hydrogels, namely CS-HMA, CS-DEAEMA, and CS-(HMA-co-DEAEMA), were synthesized by chemical crosslinking of chitosan with N-hydroxymethyl acrylamide (HMA) and 2-(diethylaminoethyl) methacrylate (DEAEMA) using glutaraldehyde and ammonium persulfate in aqueous medium. FT-IR and 1H NMR spectra confirmed successful hydrogel formation, while P-XRD revealed their crystalline characteristics. CS-(HMA-co-DEAEMA) possessed a highly porous interconnected network with the largest pore diameter (17.069 Å), which was confirmed by SEM and BET analysis. Thermal analysis demonstrated enhanced stability, with CS-(HMA-co-DEAEMA) remaining stable up to 290 °C, while rheological studies indicated superior storage modulus and yield point of LVER. Swelling studies confirmed distinct pH-responsive behaviour at pH 4.0, 7.0, and 9.0, with the CS-(HMA-co-DEAEMA) hydrogel exhibiting maximum swelling in acidic medium, suggesting suitability for the acidic tumor microenvironment. Based on these properties, CS-(HMA-co-DEAEMA) was selected for anticancer evaluation. The hydrogel exhibited significant cytotoxicity against HT-29 colorectal cancer cells (IC50 = 125.582 ± 9.118 μg/mL) with minimal toxicity toward HEK-293 normal cells. DAPI staining revealed nuclear morphological alterations, while flow cytometric analysis showed significant mitochondrial membrane potential (ΔΨM) loss, with 88.65% depolarized HT-29 cells compared to 7.28% in controls. These findings indicate that CS-(HMA-co-DEAEMA) induces mitochondrial-mediated apoptosis and highlight its potential as a promising biomaterial for further investigation in colorectal cancer therapy.

Keywords

Chitosan

;

Hydrogel

;

Rheology

;

Anticancer

;

MTT assay

;

HT-29

1. Introduction

Cancer remains a major global health challenge, with approximately 20 million new cases and 9.7 million deaths reported worldwide in 2022 [1], [2]. Colorectal cancer (CRC) is one of the most commonly diagnosed cancers and remains a major cause of cancer-related mortality, with around 1.9 million new cases and approximately 900,000 deaths reported globally [3], [4]. The increasing incidence of CRC, including the growing number of cases among younger individuals, has created a continuing need for therapeutic approaches that can improve treatment efficacy while reducing unwanted effects associated with conventional treatment strategies [5], [6]. Biomaterial-based therapeutic platforms have attracted considerable interest in this area because they can provide localized interaction with biological tissues, controlled transport of therapeutic molecules, and responsiveness to changes in the surrounding environment. Hydrogels are particularly attractive because their three - dimensional polymeric networks can retain large amounts of water and their physicochemical properties can be regulated through polymer composition and crosslinking [7], [8], [9].

Natural polymers have attracted considerable attention for the development of biomedical hydrogels because of their biocompatibility, biodegradability, structural diversity, and chemical versatility. Polysaccharides are particularly attractive owing to their renewable origin, abundance of functional groups, and ability to undergo chemical modification for specific biomedical applications [7], [10]. Their hydrophilic nature and structural adaptability have supported their development into drug-delivery systems, wound-healing materials, tissue-engineering scaffolds, and hydrogel-based platforms [8], [9], [11]. These characteristics have supported the use of polysaccharide-based hydrogels in a range of biomedical applications [7], [8], [9]. Among naturally derived polysaccharides, chitosan has received considerable attention for hydrogel fabrication. It is a cationic polysaccharide obtained from the deacetylation of chitin and contains β-(1 → 4)-linked amino and hydroxyl-bearing sugar units. The amino (-NH2) and hydroxyl (-OH) groups present along the chitosan backbone provide sites for hydrogen bonding, chemical modification, and crosslinking, which are important for the formation and stabilization of hydrogel networks [11]. Chitosan also possesses biological properties, including antimicrobial and reported anticancer activity, which make it relevant to biomedical research [12]. Its chemical reactivity and biological characteristics have led to the development of chitosan-based hydrogels with different network structures and functions. Chitosan hydrogels have been investigated for cancer-related applications because they can provide a hydrated matrix, localized interaction with biological tissues, and controlled transport of therapeutic molecules. The amino groups of chitosan can undergo protonation depending on the surrounding pH, which can influence swelling, charge density, molecular diffusion, and drug release. Chitosan-based systems have been explored in different cancer-treatment strategies, including drug and gene delivery, stimuli-responsive therapy, phototherapy, and immunotherapy [12], [13]. The properties and performance of these systems depend strongly on the hydrogel network. Crosslinking density, polymer chain interactions, porosity, and incorporation of functional components can affect mechanical strength, swelling, degradation, and biological behaviour [14]. These considerations have encouraged the development of modified chitosan hydrogels in which synthetic components are introduced to regulate the properties of the native polymer network. Recent research on chitosan-based smart hydrogels has focused on properties such as mechanical strength, swelling behaviour, structural integrity, and responsiveness to environmental stimuli [15]. Chitosan-based smart hydrogels have also been specifically investigated for colorectal cancer treatment, with reported systems focusing mainly on stimuli-responsive and localized delivery of therapeutic agents [16]. These studies indicate a shift from using chitosan simply as a biodegradable hydrogel-forming polymer toward the development of networks with controlled physicochemical and biological functions. However, the practical applications of chitosan are limited by its poor water solubility at neutral pH, low thermal stability, weak gel-forming ability, inadequate mechanical strength, and rapid degradation. Many reported systems, however, have been designed primarily as carriers for externally loaded therapeutic agents. The direct contribution of the hydrogel matrix to anticancer activity has received comparatively less attention. The incorporation of functional synthetic monomers provides a useful approach for modifying chitosan-based hydrogel networks. N-Hydroxymethyl acrylamide (HMA) contains amide and hydroxymethyl groups that can participate in hydrogen-bonding interactions within polymeric networks. These interactions can influence water uptake and the behaviour of hydrophilic hydrogel systems [17], [18], [19]. 2-(Diethylaminoethyl) methacrylate (DEAEMA) contains a tertiary amine group that can undergo protonation under acidic conditions. Changes in its protonation state can alter the charge and hydration of the polymer network, resulting in pH-dependent swelling behaviour [20]. Hydrogels containing functional monomers of this type have been investigated for stimuli-responsive and controlled-release applications [21], [22], [23]. HMA and DEAEMA provide different but complementary functionalities to a chitosan-based network. HMA can contribute hydrophilic and hydrogen-bonding interactions, whereas DEAEMA can introduce pH-responsive behaviour through its tertiary amine groups. Their combination within a chitosan network provides a rational basis for regulating the structural and environmental response of the resulting hydrogel.

Achieving a suitable balance between mechanical stability, swelling behaviour, structural integrity, and environmental responsiveness remains a challenge in chitosan-based hydrogel design. Modification with synthetic components can improve selected properties, but the resulting networks may still show limitations in structural stability or functional responsiveness [15], [16]. A hydrogel combining structural stability, pH-responsive behaviour, and intrinsic biological activity could provide a different approach to the development of chitosan-based anticancer materials. In this regard, the simultaneous incorporation of HMA and DEAEMA into a glutaraldehyde-crosslinked chitosan network represents a relevant material-design strategy. The combination of the hydrogen-bonding and hydrophilic characteristics of HMA with the pH-responsive tertiary amine functionality of DEAEMA provides an opportunity to investigate a chitosan-based hydrogel with both tunable physicochemical properties and direct biological activity. The use of HMA and DEAEMA together in a chitosan hydrogel for colorectal cancer applications has received limited attention.

In the present study, a CS-(HMA-co-DEAEMA) hydrogel was developed by incorporating N-hydroxymethyl acrylamide (HMA) and 2-(diethylaminoethyl) methacrylate (DEAEMA) into a glutaraldehyde-crosslinked chitosan network. The structural, thermal, rheological, and swelling properties of the hydrogel were investigated to understand the effect of the incorporated monomers on the chitosan network. Its biological activity was evaluated against HT-29 human colorectal adenocarcinoma cells, while HEK-293 cells were used to assess its relative cellular compatibility. The cellular response associated with the anticancer activity of the hydrogel was also investigated. We hypothesized that combining HMA and DEAEMA with chitosan would provide complementary chemical functionalities and modulate the structural and pH-responsive characteristics of the resulting hydrogel. We further hypothesized that the CS-(HMA-co-DEAEMA) hydrogel would exhibit anticancer activity against HT-29 cells with comparatively lower toxicity toward HEK-293 cells.

2. Experimental

2.1. Chemicals

Chitosan {molecular weight 17,900 Da; determined through GPC in DMF/LiCl degree of deacetylation 88% determined by using the 1H NMR [24]. Fig. S1 (Cal. S1)} was obtained from HiMedia (Mumbai, India). Acetic acid, N-hydroxymethyl acrylamide (HMA) (48 wt% aqueous solution), 2-(diethylaminoethyl) methacrylate (DEAEMA) (99%), ammonium persulfate (≥98%), glutaraldehyde (25 wt% in H2O), and potassium bromide (KBr) were purchased from Sigma-Aldrich (USA). Double-distilled water was used throughout all experiments. For cell culture, Dulbecco's Modified Eagle Medium (DMEM; CELL Clone™, India) served as the basal medium, supplemented with foetal bovine serum (FBS; Gibco, Brazil) and an antibiotic-antimycotic solution (CELL Clone™). Acridine orange (AO; HiMedia, India) and ethidium bromide (EtBr Loba Chemie, Mumbai, India) were used for AO/EtBr staining. DAPI (Sigma-Aldrich, USA), MTT (HiMedia, India), and dimethyl sulfoxide (DMSO Sigma-Aldrich, USA) were employed for viability assays. Rhodamine-123 (Rh-123, Sigma-Aldrich, USA) and 2′,7′-dichlorodihydrofluorescein diacetate (DCFH-DA, Sigma-Aldrich, USA) were used as mitochondrial potential and ROS probes, respectively. All other chemicals were of analytical grade and used without further purification.

2.2. Synthesis of hydrogel

Hydrogels with varying monomer compositions were synthesized (Table S1). For each synthesis, 0.2 g of chitosan (8.28 × 10−2 mol/L) was dispersed in 15 mL of distilled water under constant stirring. Then, 150 μL of conc. acetic acid was added dropwise until a transparent solution was obtained. The ammonium persulfate -an initiator- was added, and the solution was stirred for 15 min. Three different formulations were prepared in beakers: in the first, 200 μL of HMA (1.36 × 10−1 mol/L) was added; in the second, 200 μL of DEAEMA (6.6 × 10−2 mol/L) was used; and in the third, both 200 μL of HMA and 200 μL of DEAEMA were introduced. Finally, 50 μL of glutaraldehyde - a crosslinker was added, and the mixture was stirred further until it became viscous and gradually formed into a hydrogel (Fig. S3). All reactions were carried out under ambient conditions. After synthesizing the hydrogels, the unreacted monomers were removed using a Soxhlet extractor. The continuous circulation of distilled water (solvent) through the extraction system effectively removed residual unreacted monomers and other water-soluble impurities from the hydrogel matrix. The purified hydrogels were then dried by lyophilization, which removes water under low temperature and reduced pressure. The resulting freeze-dried hydrogels were used for all characterization studies except the rheological analysis. The degree of crosslinking (54.10%) and the degree of substitution (0.48958), by using FT-IR, have been determined (Figs. S2, S3, and Cal. S2). The molar ratio of chitosan, DEAEMA, and N-HMA in the synthesized hydrogel was calculated to be 1:0.802:1.642, and the detailed calculation is provided in Cal. S3. The synthesis process is depicted in (Fig. S3), and the inversion test is conducted on all of the hydrogels to assess their resistance to gravity-induced flow, and confirms the formation of the hydrogel (Fig. S4), while the proposed interaction mechanism is presented in (Scheme 1).

Scheme 1
  1. Download: Download high-res image (343KB)
  2. Download: Download full-size image

Scheme 1. The synthesis of CS-(HMA-co-DEAEMA) hydrogel.

2.3. Fourier transform infrared (FTIR)

FTIR spectra of chitosan (CS) and its crosslinked hydrogels were recorded in the spectral range of 4000–500 cm−1 using a JASCO Model FT/IR-4700 spectrophotometer. The hydrogel samples were ground into fine powder and compressed with potassium bromide (KBr) to form pellets, ensuring uniform transparency for infrared transmission during specimen preparation. A background spectrum of KBr was recorded prior to each measurement to ensure spectral accuracy. This analytical approach enabled the identification of characteristic functional groups in CS and its modified hydrogels, thereby confirming successful crosslinking and structural modifications [25].

2.4. NMR

Nuclear magnetic resonance (NMR) spectroscopy was used to determine the chemical composition of chitosan (CS), the monomers, and the copolymeric hydrogel. The 1H NMR spectra were obtained on a JEOL AL 500 FT-NMR spectrometer at 500 MHz and 20 °C, using deuterium oxide (D2O) and chloroform‑d (CDCl3) as solvents.

2.5. GPC (gel permeation chromatography)

Molecular weight of chitosan was determined through GPC. Gel permeation chromatography (GPC) was conducted using a high- performance liquid chromatography system (Malvern Viscotek GPCmax, Model GPC 5140) equipped with a Malvern Viscotek TDA 305 detector. The setup included detectors for light scattering (RALS at 90° and LALS at 7°), refractive index, and viscosity. The analysis was performed in DMF at 55 °C with a flow rate of 1 mL/min, utilizing a T6000M general mixed organic column (300 mm length × 8 mm inner diameter). The columns were calibrated using polystyrene (PS) standards.

2.6. Powder X-ray diffraction (P-XRD)

The crystalline and amorphous features of chitosan (CS), the monomers, and their corresponding hydrogels were analyzed using a Bruker D8 Advance (Eco) X-ray diffractometer equipped with Cu-Kα radiation (λ = 1.5418 Å). Diffraction scans were obtained at a rate of 2°/min within a 2θ range of 10–80°. The resulting diffraction profiles exhibited broad and low-intensity peaks, indicating successful copolymerization. The incorporation of HMA and DEAEMA partially disrupted the native crystalline domains of chitosan, leading to the formation of a semicrystalline hydrogel matrix. This coexistence of ordered and disordered regions was inferred to contribute to the material's mechanical flexibility [26].

2.7. Scanning electron microscopy (SEM)

For SEM analysis, the hydrogel samples were thoroughly dried to eliminate surface moisture and impurities. The specimens were subsequently cleaned using compressed air and allowed to air-dry under ambient conditions to minimize structural shrinkage. The dried hydrogels were then affixed onto metal stubs using double-sided conductive carbon tape to ensure mechanical stability and electrical conductivity during imaging. This preparation facilitated high-resolution observation of the hydrogel's surface morphology and microstructural characteristics [27].

2.8. Thermogravimetric analysis (TGA)

The thermal stability of pure chitosan (CS), CS-HMA, CS-DEAEMA, and CS-(HMA-co-DEAEMA) hydrogels was assessed using Thermogravimetric Analysis (TGA). Approximately 6 mg of each sample was placed in the instrument and heated from 50 °C to 600 °C at a constant rate of 10 °C/min under a nitrogen atmosphere to prevent oxidative degradation. The weight loss of each sample was continuously monitored as a function of temperature, and the corresponding thermograms were analyzed to elucidate the degradation behaviour and thermal resistance of the crosslinked polymeric networks [28].

2.9. Differential scanning calorimetry (DSC)

DSC was used to investigate the glass transition temperature of pure CS, CS-HMA, CS-DEAEMA, and CS-(HMA-co-DEAEMA) hydrogels. Samples were dried in a silica gel desiccator for 24 h to remove residual moisture that could interfere with the thermal signals. The DSC instrument was calibrated using an indium standard to ensure measurement accuracy. Approximately 6 mg of each dried hydrogel was sealed in an aluminium pan and heated from 30 °C to 250 °C at a rate of 10 °C/min under a nitrogen atmosphere. The heat flow curves were analyzed to identify thermal events such as glass transition, crystallisation, and melting. Transition points were determined from the intersection of tangents drawn on the slopes of the thermal peaks. These results provided insight into the structural organisation and thermal stability of the hydrogel networks [29], [30].

2.10. Swelling study

To investigate how effectively the CS, CS-HMA, CS-DEAEMA, and CS-(HMA-co-DEAEMA) hydrogels hold water, a swelling experiment using distilled water was performed under precisely controlled circumstances. The hydrogels were dried in a vacuum oven at 40 °C until they attained a consistent weight, thereby removing moisture. After drying, the samples were submerged in distilled water at 37 ± 0.1 °C and examined at different pH levels (4, 7, and 9) to assess their response to environmental changes. At regular intervals, the enlarged hydrogels were removed, gently wiped to remove surface water, and weighed. This approach continued until the swelling stabilised [31].

Swelling (%) was estimated using the following Eq. (1):(1)where Ws is the swollen hydrogel's weight, and Wo is the original dry weight.The observed swelling behaviour resembled the hydrogel's internal structure, which contains hydrophilic groups such as hydroxyl and amine, as well as the degree of crosslinking between the chitosan, HMA, and DEAEMA chains [32].

2.11. Rheology study

The rheological properties of CS, CS-HMA, CS-DEAEMA, and CS-(HMA-co-DEAEMA) hydrogels were investigated using a modular rheometer (Anton Paar MCR 702e Space) equipped with parallel-plate geometry (25 mm diameter) and a fixed gap of 1.0 mm using 0.7 mL sample in gel form. An amplitude sweep was first performed at a constant angular frequency of 10 rad/s over a strain range of 0.01–100% to determine the linear viscoelastic region (LVER). Frequency sweep tests were then conducted within the LVER at 1% strain over an angular frequency range of 0.1–100 rad/s. Storage modulus (G′) and loss modulus (G″) were recorded to assess the elastic and viscous responses of the hydrogels. Temperature sweep experiments were also carried out between 25 and 80 °C under constant strain and frequency to evaluate thermal stability and crosslinking behaviour [33].

2.12. BET analysis

To quantify nitrogen adsorption/desorption at 77.4 K, volumetric gas adsorption tests were performed using a Brunauer-Emmett-Teller (BET) surface analyzer (Quantachrome Instruments, USA, Model Autosorb IQ2) in the pressure range of 0–900 mmHg. The sample surface area and average pore size were calculated using the Barrett-Joyner-Halenda (BJH) approach. Before testing, samples were degassed overnight at 80 °C to eliminate gases, particularly bound moisture.

2.13. Assay for the anticancer activity

2.13.1. Cell culture

The HT-29 and HEK-293 cell lines were procured from the National Centre for Cell Sciences (NCCS), Pune, India. The cells were cultured in Dulbecco's Modified Eagle Medium (DMEM) supplemented with 10% fetal bovine serum (FBS), streptomycin, and penicillin. The cultures were maintained in a humidified CO2 incubator at 37 °C with 5% CO2. Approximately 1 × 106 cells were seeded in 25 cm2 culture flasks for experimental procedures. The cells were harvested for subsequent analyses upon reaching 80–90% confluency [34].

2.14. Cytotoxicity assay

2.14.1. Assessment of cell viability by MTT assay

The MTT assay is based on cellular metabolic activity. This assay utilizes the reduction of the yellow-colored tetrazolium salt, MTT, by NAD(P)H-dependent cellular oxidoreductase enzymes, which are present in metabolically active cells [35]. Normal, healthy, and rapidly growing cells show high rates of MTT reduction, converting it into an insoluble purple crystal known as formazan. In contrast, dead or inactive cells lack the necessary enzymatic activity and thus fail to produce the colored product [35]. A linear relationship is established between the number of viable cells and the amount of purple formazan produced, which allows for an accurate quantification of changes in cell proliferation or death rates [36]. The mechanism of the MTT assay is given in the supporting document.

2.15. Apoptotic studies

2.15.1. Acridine orange/ethidium bromide (AO/EB) staining

Acridine Orange/Ethidium Bromide (AO/EtBr) dual staining assay was employed to qualitatively assess cell death, allowing clear differentiation between viable, apoptotic, and necrotic cells. Acridine orange (AO), a green-fluorescent dye, penetrates both live and dead cells, whereas ethidium bromide (EtBr) selectively stains the DNA of cells with compromised membranes [37]. Early apoptotic cells are characterized by nuclear condensation, membrane blebbing and cell shrinkage. In this study, cells were treated with the CS-(HMA-co-DEAEMA) hydrogel at concentrations of 75, 125, and 175 μg/mL for 24 h. Following treatment, the cells were washed with PBS and stained with AO/EtBr staining. The characteristic apoptotic features, including cell shrinkage, membrane blebbing, and nuclear fragmentation, were then examined and documented using confocal microscopy under 40× magnification.

2.16. DAPI staining for nuclear morphology

The fluorescent dye 4′,6-diamidino-2-phenylindole (DAPI) was employed to examine nuclear changes linked to apoptosis. DAPI binds strongly to A-T-rich regions of DNA in the cells, emitting blue fluorescence. In normal healthy cells, the nucleus appears round with evenly dispersed, faint chromatin. With increasing the concentration of hydrogel CS-(HMA-co-DEAEMA, apoptotic cells display clear morphological hallmarks, including chromatin condensation (pyknosis), observed as bright, compact fluorescent masses, and nuclear fragmentation, resulting in the formation of apoptotic bodies [38]. These characteristic features make DAPI staining a dependable method for detecting apoptotic cells [39].

2.17. Estimation of ROS (reactive oxygen species) generation

Intracellular reactive oxygen species (ROS) were assessed using the 2′,7′-dichlorodihydrofluorescein diacetate (DCFH-DA) assay. This non-fluorescent, cell-permeable probe easily diffuses across the plasma membrane, where intracellular esterases break down the acetate groups to transform it into the polar, non-fluorescent form 2′,7′-dichlorodihydrofluorescein (DCFH), which effectively traps the probe inside the cell. In the presence of ROS such as hydroxyl and peroxyl radicals, DCFH is rapidly oxidized to form 2′,7′-dichlorofluorescein (DCF), a highly fluorescent compound [40]. In the presence of ROS such as hydroxyl and peroxyl radicals, DCFH is oxidized to form 2′,7′-dichlorofluorescein (DCF), a highly fluorescent compound. The intensity of the resulting green fluorescence directly reflects the intracellular ROS levels, enabling visual detection of oxidative stress [41].

2.18. Mitochondrial membrane potential ()

The loss of mitochondrial membrane potential (ΔΨm) represents a critical indicator of the intrinsic apoptotic pathway and serves as an essential parameter for evaluating cellular health. JC-1 staining was employed as a reliable method to assess changes in ΔΨm. In depolarized mitochondria, JC-1 exists in its monomeric form within the cytoplasm and emits green fluorescence, whereas in healthy mitochondria with preserved ΔΨm, it forms red-orange fluorescent aggregates. This distinct red-to-green fluorescence shift is largely independent of mitochondrial mass or cell number, providing a definitive and quantifiable measure of mitochondrial dysfunction [42].

To evaluate the effect of the CS-(HMA-co-DEAEMA) hydrogel on mitochondrial integrity, HT-29 cells were seeded in 6-well culture plates at a density of 1 × 105 cells per well and allowed to adhere for 24 h. The cells were subsequently exposed to varying concentrations of the hydrogel for 24 h at 37 °C in a humidified incubator containing 5% CO2. Following treatment, the cells were rinsed with phosphate-buffered saline (PBS) and stained with JC-1 dye (1 μM) for 30 min in the dark at room temperature. The fluorescence patterns were then examined using a confocal laser scanning microscope to assess alterations in mitochondrial membrane potential.

3. Results and discussion

3.1. FTIR analysis

FTIR spectroscopy was employed to confirm the copolymerization of chitosan (CS) with N-(Hydroxymethyl) acrylamide (HMA) and 2-(Diethylaminoethyl) Methacrylate (DEAEMA), and to investigate structural changes in the resulting hydrogels (Figs. 1 and S7-S9). The FTIR spectrum of chitosan (Fig. S1) exhibited a broad band around 3465 cm−1, corresponding to overlapping -OH and -NH2 stretching vibrations, along with a characteristic amide-I (C=O) band at 1653 cm−1 and -C-H band at 2883 cm−1. Peaks observed at 1431 and 1373 cm−1 were attributed to CH2 bending, while Csingle bondO and C-O-C stretching vibrations appeared near 1151 and 1020 cm−1, respectively, confirming the saccharide backbone [43]. DEAEMA (Fig. S7) showed peaks at 2925 cm−1 (aliphatic Csingle bondH), 1722 cm−1 (ester Cdouble bondO), and 1631 cm−1 (vinyl Cdouble bondC), along with a Csingle bondN stretch at 1170 cm−1, characteristic of methacrylate groups. HMA (Fig. S8) exhibited a broad -OH/-NH2 band at 3335 cm−1, with amide Cdouble bondO at 1655 cm−1, Csingle bondN at 1239 cm−1, and Csingle bondO near 1044 cm−1, indicating its acrylamide framework. Upon hydrogel formation (Fig. 1), notable spectral shifts were recorded. In the CS-DEAEMA hydrogel, the broad hydrogen-bonded -OH and -NH2 peak was observed at 3483 cm−1, indicating increased intra-network interactions. The Cdouble bondO stretching peak appears to 1730 cm−1, Csingle bondH appears at 2925 cm−1, Cdouble bondN at 1643 cm−1, -CH2 at 1412 cm−1 and 1325 cm−1, -C-N and -CO at 1157 cm−1, C-O-C at 1036 cm−1, and the absence of the vinyl Cdouble bondC peak confirmed successful polymerization. The CS-HMA hydrogel demonstrated similar modifications with a red-shifted -OH/-NH2 band at 3437 cm−1, -CO, Cdouble bondO stretch at 1660 cm−1, and appearance of Csingle bondO and C-O-C bands at 1064 and 1016 cm−1, respectively [44].

Fig. 1
  1. Download: Download high-res image (415KB)
  2. Download: Download full-size image

Fig. 1. FT-IR spectra of synthesized hydrogels: CS-DEAEMA, CS-HMA, CS-(HMA-co-DEAEMA).

The copolymeric hydrogel CS-(HMA-co-DEAEMA) revealed a merged spectral signature with an intense hydrogen-bonding broad band at 3460 cm−1, -C-H at 2925 cm−1, and ester Cdouble bondO stretching at 1729 cm−1. The band at 1643 cm−1 was assigned to the imine (C=N) stretching vibration formed between the amino groups of chitosan and the aldehyde groups of glutaraldehyde, confirming successful crosslinking of the hydrogel network. The disappearance of the monomeric vinyl peaks and emergence of Csingle bondO and C-O-C absorptions at 1049 and 1034 cm−1 confirmed the formation of an interpenetrating polymer network of HMA and DEAEMA, respectively, on chitosan [45].

The emergence of ester and amide functionalities, along with the disappearance of the vinyl bond, and the presence of the Cdouble bondN stretching band arising from glutaraldehyde-mediated crosslinking, further confirmed the formation of a robust, interpenetrated crosslinked hydrogel network with responsive and hydrophilic functional groups suitable for biomedical and environmental applications [46].

3.2. NMR analysis

The synthesis of the CS-(HMA-co-DEAEMA) hydrogel was validated by 1H NMR analysis, which revealed typical proton signals for chitosan, N-HMA, DEAEMA, and glutaraldehyde moieties (Figs. 2 and S10-S11). The resonance signal observed at δ 4.4 ppm (‘a’) was assigned to the proton of the chitosan backbone (-CH), indicating the presence of the polysaccharide structure within the hydrogel matrix [47]. The peak appearing at δ 3.3 ppm (‘b’) corresponds to the methylene protons (-CH2) adjacent to the hydroxyl group of N-HMA. The characteristic methyl proton adjacent to -NCH2 of DEAEMA was detected at δ 1.3 ppm (‘c’). A resonance peak at δ 1.2 ppm (‘d’) was assigned to methylene protons associated with glutaraldehyde crosslinking segments. The peak appears at δ 1.1 ppm (‘e’) associated with chitosan, while the signal at δ 4.7 ppm (‘f’) was attributed to the methylene protons of DEAEMA [48]. Additionally, the signal observed at δ 4.9 ppm (‘g’) corresponds to methylene protons of chitosan, further supporting the retention of the chitosan framework after crosslinking and polymerization. The peak appeared at δ 3.9 ppm (‘h’) associated with the methine (-CH) proton of chitosan.

Fig. 2
  1. Download: Download high-res image (326KB)
  2. Download: Download full-size image

Fig. 2. 1H NMR spectra of CS-(HMA-co-DEAEMA) hydrogel.

Overall, the presence of these characteristic chemical shifts confirms the successful integration of N-HMA, DEAEMA, and glutaraldehyde with chitosan, resulting in a chemically crosslinked CS-(HMA-co-DEAEMA) copolymer hydrogel network.

3.3. P-XRD analysis

Powder X-ray diffraction (XRD) analysis was used to evaluate the crystallinity and structural modifications of the synthesized materials (Fig. S12). Pure chitosan showed characteristic peaks at 2θ = 14.46° and 16.67°, corresponding to its crystalline nature derived from the regular hydrogen-bonded arrangement of polysaccharide chains. These findings are consistent with earlier reports that relate chitosan crystallinity to its extensive hydrogen-bonding network [49]. The DEAEMA monomer displayed a broad peak at 18.11°, confirming its predominantly amorphous nature, typical of flexible vinyl monomers [50]. Likewise, HMA exhibited a broad peak at 16.99°, suggesting an amorphous structure with weak short-range ordering from amide group interactions [51], [52]. Notable changes were observed upon hydrogel formation. In the CS-DEAEMA hydrogel, the characteristic chitosan peaks shifted slightly to 16.75°, while additional peaks appeared at 30.76° and 40.77°. These shifts indicate disruption of native hydrogen bonding and the creation of new amorphous domains due to DEAEMA incorporation and radical polymerization [53]. The CS-HMA hydrogel showed prominent peaks at 30.63° and 40.41°, with the disappearance of peaks in the 14–18° region, reflecting a major loss of native chitosan crystallinity. This disruption can be attributed to interactions between chitosan hydroxyl groups and the hydrocarbon segments of HMA, generating new crosslinked amorphous networks.

The CS-(HMA-co-DEAEMA) hydrogel exhibited combined features, with peaks at 18.10°, 30.18°, and 40.21°. Retention of the 18.10° peak suggests some residual chitosan ordering, while the new peaks confirm the formation of amorphous domains through synergistic crosslinking involving both DEAEMA polymerization and HMA bonding. In Fig. S4, the XRD patterns demonstrate that the monomer incorporation and crosslinking substantially modified the crystallinity of chitosan, transforming the hydrogels into amorphous, interpenetrated network structures [54], [55].

3.4. SEM study

The surface morphology of CS-HMA, CS-DEAEMA, and CS-(HMA-co-DEAEMA) hydrogels was examined by scanning electron microscopy (SEM). As shown in (Fig. 3(a-d)) all hydrogels exhibited a porous, heterogeneous structure composed of interconnected micro and macropores of varying sizes [56]. This porous network arises mainly from phase separation during hydrogel formation and subsequent freeze-drying, where water sublimation leaves voids within the polymer matrix. The incorporation of DEAEMA introduces flexible, pH-responsive domains, while HMA contributes hydrophobic interactions that promote microphase separation, collectively stabilising pore formation. Owing to their lightweight and porous nature, the freeze-dried hydrogels were stable enough to rest on delicate surfaces, as illustrated in (Fig. 3(e)). Overall, the SEM analysis confirmed the successful formation of structurally stable and highly porous hydrogel networks. In addition, the surface area and pore diameter of the synthesized hydrogels were evaluated using BET analysis (Figs. S15-S20 and Table S6). The BET surface area of CS-DEAEMA HG, CS-HMA HG, and CS-(HMA-co-DEAEMA) HG was determined to be 8.438, 3.201, and 9.905 m2g−1, respectively (Figs. S15, S17, and S19). Furthermore, the average pore diameters of CS-DEAEMA HG, CS-HMA HG, and CS-(HMA-co-DEAEMA) HG were found to be 17.043, 15.260, and 17.069 Å, respectively (Figs. S16, S18, S20 and Table S6). The comparatively higher surface area and pore diameter of the copolymeric hydrogel indicate the development of a more interconnected porous architecture, which may facilitate enhanced diffusion/adsorption performance, binding, swelling behaviour, mechanical strength, and the availability of active sites for biomedical and environmental applications [57].

Fig. 3
  1. Download: Download high-res image (244KB)
  2. Download: Download full-size image

Fig. 3. a-c) Scanning electron micrographs of CS-HMA, CS-DEAEMA, and CS-(HMA-co-DEAEMA) hydrogels at 10, 20 and 10 μm magnification, respectively, d) Scanning electron micrographs of CS-(HMA-co-DEAEMA) hydrogels at 1 μm magnification, e) a block of freeze-dried CS-(HMA-co-DEAEMA) hydrogel standing on a flower portulaca.

3.5. TGA

Thermogravimetric analysis (TGA) was used to assess the thermal stability and degradation behaviour of chitosan and its modified hydrogel systems (Fig. 4 and Table S2). Pristine chitosan (CS) follows a three-step degradation profile. The initial degrading process at 57–114 °C involves the elimination of physically adsorbed and bound water. The second main stage at 221–397 °C results in considerable mass loss owing to glycosidic linkage breakage and pyranose ring structure cleavage, suggesting polymer backbone collapse [58]. The third phase at 400–589 °C results in progressive carbonization and the production of residual char ~27.5%.

Fig. 4
  1. Download: Download high-res image (154KB)
  2. Download: Download full-size image

Fig. 4. The effect of temperature on % residual mass of chitosan and its hydrogels- CS-HMA, CS-DEAEMA, CS-(HMA-co-DEAEMA), respectively.

When chitosan is modified with N-HMA, the thermal behaviour is changed. Due to combined moisture removal and methylol dehydration, pure N-HMA (Fig. S13) itself exhibits an early and significant weight loss ~40% at 62–185 °C, followed by condensation reactions and ultimately backbone disintegration at 188–247 °C, leaving char residue (~26%), indicating a carbon-forming propensity at 252–325 °C. However, a four-step breakdown pattern is shown when HMA was added to chitosan (CS-HMA). The hydrogel network's improved water retention is seen in the first stage at 60–150 °C. Successful crosslinking is confirmed by the second step, which occurs at 173–260 °C and is attributable to methylol group condensation and dehydration. The breakdown of the chitosan backbone and acrylamide-like fragment occurs in the third stage at 256–362C [59]. In comparison to pristine chitosan, the last step at 379–504 °C corresponds to the development of aromatic or imide-like structures, which results in a much greater char yield (~39%). This suggests that the synthesis of crosslinked networks has increased thermal stability.

The TGA profile of DEAEMA (Fig. S13) demonstrates a single, fast mass loss event about ~100 °C, with no multistep degradation trend. This phenomenon may be due to the volatilization of the low molecular weight liquid monomer, not heat breakdown. DEAEMA may not undergo stepwise bond breakage because it lacks a polymeric or crosslinked backbone, and instead evaporates virtually entirely, leaving negligible residue. This contrasts with the multistage degradation shown in the CS-DEAEMA hydrogel. A three-step degradation pattern is shown in the case of CS-DEAEMA. At 61–133 °C, the first step is associated with the loss of bound water; at 174–340 °C, the second stage is associated with the breakage of diethylamino side chains, releasing volatile fragments. The methacrylate backbone and chitosan structure degrade simultaneously in the last step, which occurs between 352 and 510 °C. The total char yield is around 26.73%.

The copolymer hydrogel CS-(HMA-co-DEAEMA) has a mixed degradation profile driven by both the HMA and DEAEMA monomers. The first degrading process occurs when bound water evaporates at temperatures ranging from 57 to 106 °C [60]. The second degradation stage, which occurs at 123–290 °C, consists of overlapping processes such as methylol dehydration and diethylamino group breakage. This is followed by a large disintegration step at 289–392 °C, during which both the polysaccharide and vinyl polymer backbones are broken down simultaneously. The last stage is carbonization at 402–527 °C, and the char yield is about 23%. Overall, the thermal stability of the samples follows the sequence. DEAEMA < N-HMA < CS-(HMA-co-DEAEMA) < CS-DEAEMA < CS < CS-HMA.

3.6. DSC analysis

DSC analysis was conducted to investigate the glass transition temperature of chitosan and its hydrogels between 25 and 250 °C, as shown in (Fig. 5). All samples exhibited a low-temperature endotherm corresponding to the loss of free and hydrogen-bonded water, consistent with their hygroscopic nature. The dehydration peak varied systematically with CS-DEAEMA, which displayed the lowest transition at 92.3 °C, followed by CS-(HMA-co-DEAEMA) at 104.8 °C and pure chitosan at 106.4 °C, while CS-HMA exhibited the highest temperature at 114.4 °C. The upward shift in CS-HMA is attributed to enhanced hydrogen bonding via hydroxymethyl and amide functionalities, which increase bound-water content and require higher energy for removal. In contrast, DEAEMA incorporation reduced the transition temperature, reflecting weaker hydrogen bonding and greater chain mobility due to hydrophobic ethyl groups and tertiary amines. The copolymer hydrogel exhibited intermediate behaviour, balancing HMA-driven water binding and DEAEMA-driven plasticization [61]. These findings suggest that HMA-rich networks confer greater wet/thermal stability, whereas DEAEMA-rich systems enhance swelling responsiveness under physiological conditions.

Fig. 5
  1. Download: Download high-res image (142KB)
  2. Download: Download full-size image

Fig. 5. The effect of temperature on phase change of chitosan and its hydrogels- CS-HMA, CS-DEAEMA, CS-(HMA-co-DEAEMA).

3.7. Swelling behaviour study

The Donnan equilibrium, which controls the ionic balance between the hydrogel matrix and the surrounding media, is the main factor influencing the swelling behaviour of chitosan-based hydrogels. Water intake is driven by osmotic pressure, which is created when fixed charges along the polymer chains attract counter-ions. Therefore, the ionisation of functional groups within the hydrogel network, which fluctuates with pH, determines the degree of swelling [62]. The pure CS hydrogel shows comparatively less swelling (Fig. S14) because of its smaller pH-responsive range and fewer ionisable groups.

The protonation of chitosan and DEAEMA's amino groups causes all hydrogels to swell considerably at pH 4.0, which results in considerable electrostatic repulsion between positively charged sites. The order in which the swelling occurs is CS < CS-HMA < CS-DEAEMA < CS-(HMA-co-DEAEMA). Because of its hydrophobic nature, which restricts water diffusion, CS-HMA swells the least. As protonated tertiary amines increase osmotic pressure, CS-DEAEMA expands more, but the copolymer hydrogel shows the most swelling due to the combination action of hydrophilic-hydrophobic balance and a large number of ionisable groups. In accordance with CS < CS-HMA < CS-DEAEMA < CS-(HMA-co-DEAEMA), the swelling capacity of all hydrogels achieves its maximum at pH 7.0, as shown in (Fig. 6). Hydrophilic domains have a significant interaction with water molecules at this neutral state, although partial protonation is maintained. Because of the combined effects of DEAEMA and HMA, the copolymer exhibits superior swelling. The sequence changes to CS < CS-DEAEMA < CS-(HMA-co-DEAEMA) < CS-HMA at pH 9.0. Deprotonating amino groups lowers the fixed charge density in alkaline environments, which lessens the Donnan effect. Because of its hydroxyl and amide groups, which maintain water contacts, CS-HMA displays the most swelling, whereas CS-DEAEMA shows the least because of loss of ionisation. In conclusion, the swelling behaviour of chitosan-based hydrogels is strongly influenced by pH, showing maximum expansion in acidic conditions, followed by moderate swelling at neutral pH due to protonation, and minimal swelling in alkaline conditions. HMA and DEAEMA together offer tunable swelling appropriate for drug administration and controlled release applications, while DEAEMA improves responsiveness.

Fig. 6
  1. Download: Download high-res image (240KB)
  2. Download: Download full-size image

Fig. 6. A plot showing pH-dependent swelling behaviour of CS-HMA, CS-DEAEMA, and CS-(HMA-co-DEAEMA) hydrogels at pH 4.0, 7.0 and 9.0.

3.8. Rheology study

3.8.1. Frequency sweep test

To assess the mechanical and viscoelastic behaviour of different chitosan-based hydrogel formulations under oscillatory stress, a frequency sweep test was performed. This test evaluates the material's capacity to store and release energy by revealing how it reacts to deformation over a variety of frequencies [63]. Important rheological parameters were measured to ascertain each sample's elastic and viscous properties, including storage modulus, loss modulus, complex modulus, and loss factor. The complex modulus can be calculated by Eq. (2):(2)where,

  • G⁎ = Complex modulus,

  • G′ = Storage modulus,

  • G″ = Loss modulus.

The pure chitosan hydrogel has a very low storage modulus and a high loss factor, indicating viscous-dominant behaviour with poor elastic recovery. The high Tan δ value (>1) indicates that most mechanical energy is wasted rather than retained, indicating a weak internal network, low mechanical integrity, and even shows a viscous dominant structure having a crossover point at 63.66 Pa. The CS-DEAEMA hydrogel has a high storage modulus (G′ = 6525 Pa) and a low Tan δ (0.043), suggesting a robust elastic network with minimum energy dissipation. This improvement is attributed to DEAEMA's hydrophobic ethyl chains and methacrylate groups, which encourage chain tangling and covalent crosslinking. The CS-HMA hydrogel outperformed the pure CS hydrogel in terms of elasticity (G′ = 5373 Pa, Tan δ = 0.147). This was due to the hydroxymethyl (-CH2OH) groups of HMA, which allow for hydrogen bonding and physical crosslinking, strengthening the gel structure. The CS-(HMA-co-DEAEMA) hydrogel had the largest storage modulus (G′ = 9161 Pa) and lowest Tan δ (0.065), suggesting greater mechanical strength and elastic behaviour as shown in (Fig. 7) and (Table S3). The synergistic effect of DEAEMA and HMA improves crosslinking and bonding, yielding a robust, deformation-resistant network ideal for dynamic circumstances.

Fig. 7
  1. Download: Download high-res image (238KB)
  2. Download: Download full-size image

Fig. 7. Frequency sweep measurement of hydrogels- CS, CS-DEAEMA, CS-HMA, and CS-(HMA-co-DEAEMA) in terms of storage modulus and loss modulus as a function of angular frequency.

3.8.2. Amplitude sweep study

To assess the structural integrity and viscoelastic behaviour of chitosan-based hydrogels under increasing strain, an amplitude sweep test was performed. The test determines the yield point, crossover point, and Linear Viscoelastic Region (LVER), which together show how well the hydrogel structure withstands deformation. According to (Table S4), the CS hydrogel showed an early crossover point at 48.03% strain and a very narrow LVER (G′ = 3.23 Pa; G″ = 3.16 Pa), which suggests poor mechanical stability and a weak gel network that disintegrates under low deformation [64]. As a result of the addition of DEAEMA, the CS-DEAEMA hydrogel demonstrated enhanced elasticity and network strength, as evidenced by a wider LVER, a delayed crossover point (21.92% strain), and a higher G′ (10.41 Pa). With moderate moduli and a crossover at 21.23% strain, the CS-HMA hydrogel demonstrated intermediate performance, indicating that HMA reinforced it but not as well as DEAEMA. Out of all the formulations, the CS-(HMA-co-DEAEMA) hydrogel showed the strongest viscoelastic properties. It featured a G′ of 10.75 Pa, the broadest LVER, the greatest yield point (15.13% strain), and a delayed crossover point at 31.85% strain, as shown in (Fig. 8) and (Table S4). These features demonstrate a potent synergistic interaction between DEAEMA and HMA, resulting in a robust and well-organised hydrogel network that can withstand structural degradation at elevated strain levels. For applications needing structural integrity and mechanical robustness, this formulation is consequently the most appropriate.

Fig. 8
  1. Download: Download high-res image (181KB)
  2. Download: Download full-size image

Fig. 8. Amplitude sweep measurement of hydrogels CS-DEAEMA, CS-HMA, and CS-(HMA-co-DEAEMA) in terms of storage modulus and loss modulus as a function of strain.

3.8.3. Temperature ramp

A temperature ramp rheological investigation was performed to assess the temperature-dependent viscoelastic behaviour of the chitosan-based HMA-DEAEMA hydrogels as shown in (Fig. 9) and (Table S5). Throughout the temperature range, the storage modulus (G′) remained higher than the loss modulus (G″), showing that the hydrogel maintained its elastic-dominant, solid-like character without transitioning to gel-sol. Tan δ (G″/G′) values remained below unity at all tested temperatures, showing robust gel-like behaviour and no major structural disintegration [65]. The hydrogel's thermal resistance and viscoelastic stability under heat stress were demonstrated by the absence of a crossover point between G′ and G″. These findings indicate that the composite hydrogel is structurally robust and well-suited for biological and environmental applications requiring temperature resistance.

Fig. 9
  1. Download: Download high-res image (202KB)
  2. Download: Download full-size image

Fig. 9. Temperature ramp measurement of hydrogels-CS, CS-DEAEMA, CS-HMA, and CS-(HMA-co-DEAEMA) in terms of storage modulus and loss modulus as a function of temperature.

In comparative studies, while the CS-DEAEMA hydrogel showed slightly higher temperature-responsive viscoelastic properties than the CS-(HMA-co-DEAEMA) system, the incorporation of DEAEMA into the chitosan-HMA hydrogel still significantly enhanced mechanical strength compared to the CS-HMA and pure chitosan-based hydrogels. This improvement can be attributed to the chemical and physical contributions of the DEAEMA monomer. The hydrophobic ethyl chains of DEAEMA promote hydrophobic interactions and increased polymer chain entanglement, contributing to enhanced stiffness. Meanwhile, the methacrylate group (C=C) of DEAEMA participates in covalent crosslinking during polymerization, reinforcing the hydrogel network. Additionally, the protonation-deprotonation ability of DEAEMA's tertiary amine groups imparts pH-responsive swelling behaviour, while ionic interactions and secondary bonding within the matrix further improve the network integrity [66]. These synergistic features provide the CS-(HMA-co-DEAEMA) hydrogel with the dual advantage of environmental sensitivity and tunable mechanical properties, making it more effective than hydrogels constructed only from chitosan or HMA. (Table S5) shows that the temperature range of 25 °C to 50 °C marks the region where rheological parameters begin to change notably. A gradual decline in both storage modulus (G′) and loss modulus (G″) is observed starting around 30 °C, continuing through to 50 °C, indicating the onset of thermal softening of the hydrogel network. Correspondingly, Tan δ values exhibit a slight increase within this range, reflecting enhanced chain mobility and viscoelastic behaviour with rising temperature. According to all the results, the CS-(HMA-co-DEAEMA) hydrogel is the potential candidate for biomedical applications because of its exceptional structural stability, swelling behaviour, and mechanical strength. Therefore, we selected this optimized hydrogel to evaluate its anticancer activity as a practical application ahead.

3.9. Hydrogel decreased the cell viability of HT-29 colorectal cancer cells

The antitumor potential of CS-HMA, CS-DEAEMA, and CS-(HMA-co-DEAEMA) was evaluated against HT-29 colorectal cancer cells using the standard MTT assay (3-(4,5-dimethylthiazol-2-yl)-2,5-diphenyltetrazolium bromide), a colorimetric method that measures cellular metabolic activity and indirectly reflects [67]. HT-29 cells (1 × 104 cells per well) were seeded into 96-well ELISA plates and incubated for 24 h to allow attachment. The cells were then exposed to increasing concentrations (0, 25, 50, 75, 100, 125, 150, 175, 200, 225, and 250 μg/mL) of each hydrogel formulation, followed by assessment of cell viability.

The results (Fig. 10(a-c)) demonstrated that all three hydrogels reduced the viability of HT-29 cells in a dose-dependent manner when compared with the untreated control. The calculated IC50 values indicated that CS-(HMA-co-DEAEMA) exhibited stronger cytotoxic activity (125.582 ± 9.118 μg/mL) than CS-HMA (231.820 ± 5.600 μg/mL) and CS-DEAEMA (186.266 ± 4.582 μg/mL), achieving significant growth inhibition at comparatively lower concentrations. These findings suggest that CS-(HMA-co-DEAEMA) possesses superior antiproliferative potential against HT-29 cells. To further examine the safety profile of CS-(HMA-co-DEAEMA), cytotoxicity was also evaluated in normal human embryonic kidney cells (HEK-293) using the same MTT assay protocol. The results in (Fig. 10(d)) showed that CS-(HMA-co-DEAEMA) did not significantly affect the viability of HEK-293 cells, indicating good biocompatibility.

Fig. 10
  1. Download: Download high-res image (613KB)
  2. Download: Download full-size image

Fig. 10. The bar graph shows how a) CS-HMA, b) CS-DEAEMA, c) CS-(HMA-co-DEAEMA) affected the viability of HT-29 cells, d) HEK-293 cells at various concentrations ranging from 0, 25, 50, 75, 100, 125, 150, 200, 225, and 250 μg/ml throughout the duration of a 24-hour treatment. The findings are representative, considering the mean ± SD of three different tests shows that *p < 0.05, **p < 0.01, ***p < 0.001 when compared to the control.

The enhanced and selective cytotoxicity of the CS-(HMA-co-DEAEMA) copolymer against HT-29 cells is driven by a synergistic biophysical mechanism. Cancer cells, including HT-29, possess a significantly more negatively charged surface compared to normal cells (such as HEK-293) due to altered glycolysis and the overexpression of anionic molecules such as sialylated glycans. Concurrently, the tumor microenvironment is typically mildly acidic (pH ~6.5–6.8).

The inclusion of DEAEMA provides pendant tertiary amine groups that undergo rapid protonation in this acidic environment, generating a strong positive charge. This facilitates highly targeted electrostatic attraction and subsequent membrane disruption specifically against the negatively charged HT-29 cells. Meanwhile, the HMA component provides essential structural stability, hydrogen bonding, and a porous interconnected network (as evidenced by our SEM data), which maximizes the surface contact area between the protonated hydrogel and the cancer cell membrane. The single-monomer hydrogels (CS-HMA and CS-DEAEMA) lack this optimal balance of high cationic charge density and structural resilience, resulting in comparatively lower cytotoxicity. In summary, CS-(HMA-co-DEAEMA) demonstrated marked antitumor efficacy against HT-29 cells while maintaining minimal toxicity toward normal cells, highlighting its promise as a potential therapeutic candidate.

3.10. CS-(HMA-co-DEAEMA) induces apoptosis in HT-29 cells

Determining the anticancer potential of CS-(HMA-co-DEAEMA) requires the detection of apoptosis (programmed cell death), which is crucial in the cell death of cancer cells. Following a 24-hour treatment period (0, 75, 125, and 175 μg/mL), dual acridine orange/ethidium bromide (AO/EtBr) staining was carried out to examine whether CS-(HMA-co-DEAEMA) causes apoptosis in HT-29 cells. In order to differentiate between viable, early apoptotic, and late apoptotic cells, ethidium bromide only enters cells with damaged membranes and stains them orange to red. Acridine orange, on the other hand, penetrates all cells and fluoresces green [68].

The cells in the untreated control group showed consistent green fluorescence and showed no signs of apoptosis, indicating that they were viable. However, HT-29 cells treated with CS-(HMA-co-DEAEMA) displayed distinct morphological alterations that are indicative of apoptosis. Numerous cells displayed yellowish-green fluorescence at lower concentrations, along with chromatin condensation and mild membrane disruption, which suggested the start of early apoptosis. The cells showed more noticeable nuclear condensation, DNA fragmentation, and orange-red fluorescence, all of which are indicative of late-stage apoptosis, as the concentrations increased [69]. These findings support the potential of CS-(HMA-co-DEAEMA) as an anticancer agent by showing that it efficiently and concentration-dependently induces apoptosis in HT-29 cells, as shown in (Fig. 11).

Fig. 11
  1. Download: Download high-res image (368KB)
  2. Download: Download full-size image

Fig. 11. Confocal images of HT-29 cells stained with acridine orange/ethidium bromide (AO/EtBr) after 24 h of treatment with CS-(HMA-co-DEAEMA). At 40× magnification, healthy cells appear green, early apoptotic cells show yellowish-green with condensed nuclei, and late apoptotic cells appear orange-red with fragmented nuclei. (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.)

Mechanistically, the hydrogel kills cancer cells by triggering severe oxidative stress. It generates a dose-dependent spike in ROS that damages the mitochondria, evidenced by the membrane depolarization seen in 88.65% of treated HT-29 cells. This depolarization activates the intrinsic apoptotic pathway, leading to the DNA fragmentation and nuclear condensation observed in our staining [70]. Ultimately, this ROS-driven mitochondrial failure is the primary driver of the hydrogel's selective toxicity against colorectal cancer cells.

While our HEK-293 results demonstrate initial biocompatibility, advancing this hydrogel requires broader testing. Future in vitro safety studies should include L929 fibroblasts and PBMCs to evaluate localized and blood compatibility [71]. For in vivo translation, tumor-bearing mouse models are ideal for assessing both systemic toxicity and targeted efficacy. Finally, evaluating the hydrogel's environmental impact is essential [72]; aquatic models like embryonic zebrafish and Daphnia magna offer excellent, rapid platforms for assessing overall ecotoxicity and developmental safety [73].

3.11. CS-(HMA-co-DEAEMA) generates apoptosis by alter morphology and DNA fragmentation in HT-29 Cells

To determine the nuclear alterations associated with apoptosis, HT-29 cells were stained with DAPI (4′,6-diamidino-2-phenylindole), a blue fluorescent dye that exhibits a significant affinity for A-T-rich regions of DNA. In untreated control cells, the nuclei exhibited a smooth, rounded morphology and uniform staining, indicating an absence of chromatin damage. Conversely, cells exposed to CS-(HMA-co-DEAEMA) for 24 h exhibited distinct characteristics of apoptosis, such as chromatin condensation and nuclear disintegration. The alterations were evident in the enhanced and punctate DAPI fluorescence detected in the treated cells [74]. In comparison to the control group, a significantly higher quantity of HT-29 cells shows DAPI positivity after treatment, confirming that CS-(HMA-co-DEAEMA) causes apoptosis through modifications in nuclear morphology, as shown in (Fig. 12).

Fig. 12
  1. Download: Download high-res image (372KB)
  2. Download: Download full-size image

Fig. 12. Effects of CS-(HMA-co-DEAEMA) on HT-29 cells. DAPI staining shows nuclear changes after treatment at different concentrations compared with the control, observed under Confocal microscopy (20×). Treated cells displayed condensed and fragmented nuclei, typical of apoptosis.

3.12. CS-(HMA-co-DEAEMA) induces apoptosis by enhancing reactive oxygen species (ROS) production

In apoptosis, reactive oxygen species (ROS) assume as a vital role. At modest doses, they facilitate the proliferation, viability, and metabolic modification of cancer cells. Excessive oxidative stress induced by reactive oxygen species can damage DNA, alter cellular functioning, and ultimately initiate apoptosis. Reactive oxygen species (ROS) are a significant focus in cancer therapy due to their dualistic properties. The present study investigated the potential of CS-(HMA-co-DEAEMA) to enhance ROS generation in HT-29 cells. After a 24-hour incubation with different doses of the chemical, the cells were stained with DCFDA, a fluorescent probe that emits green light upon interaction with reactive oxygen species (ROS) in the cell. Fig. 4 indicates that untreated control cells exhibited minimal green fluorescence, signifying low basal ROS levels. In contrast, treated cells exhibited a clear increase in fluorescence intensity that was dependent on concentration. At concentrations of 75, 125, and 175 μM, the effect was observed, signifying a substantial elevation in ROS generation. The amplified ROS levels are caused by the specific pathway of the copolymer inside the cell. Once within acidic endosomes, the amine groups of DEAEMA act as a ‘proton sponge’ to swell and rupture the endosomal compartment, releasing the hydrogel into the cytosol. The copolymer is highly positively charged and thus strongly attracted to the negatively charged mitochondria. This interaction physically disrupts the electron transport chain, causing a massive release of ROS.

These data indicate that CS-(HMA-co-DEAEMA) induces oxidative stress and death in cancer cells by elevating ROS levels beyond safe limits, hence facilitating its anticancer actions as shown in (Fig. 13).

Fig. 13
  1. Download: Download high-res image (332KB)
  2. Download: Download full-size image

Fig. 13. ROS generation detected by DCFH-DA staining after 24 h treatment with 75, 125, and 175 μg/mL, observed under confocal microscopy (40×). Treated cells showed stronger green fluorescence, indicating higher ROS levels than the control. (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.)

3.13. CS-(HMA-co-DEAEMA) treatment down-regulate mitochondrial membrane potential (ΔΨm) in HT-29 cells

Mitochondria are one of the main controllers of apoptosis, and a change in the mitochondrial membrane potential (ΔΨM) is a key sign that the mitochondria are incapable of functioning properly. To assess the impact of CS-(HMA-co-DEAEMA) on mitochondrial integrity in HT-29 cells, JC-1 labelling was performed and analyzed using confocal microscopy. When JC-1 developed in the mitochondrial matrix of healthy control cells, it made red J-aggregates. The observable shift in fluorescence from red to green in cells treated with CS-(HMA-co-DEAEMA) showed that JC-1 monomers were present in the cytoplasm because the membrane was depolarised. Quantitative analysis (Fig. 14(a)) indicates that the red/green fluorescence ratio in treated cells was significantly diminished compared to controls (p < 0.001). Flow cytometry confirmed these results. A notable reduction in ΔΨM was noted, with cells treated with CS-(HMA-co-DEAEMA) displaying depolarisation in 88.65% of cases, while control cells demonstrated similar effects in only 7.28% of cases (Fig. 14(b)). All of these results back up the idea that CS-(HMA-co-DEAEMA) has an effect on mitochondria, which causes HT-29 cells death.

Fig. 14
  1. Download: Download high-res image (185KB)
  2. Download: Download full-size image
Fig. 14
  1. Download: Download high-res image (246KB)
  2. Download: Download full-size image

Fig. 14. a: Confocal images of HT-29 cells stained with JC-1 to assess mitochondrial membrane potential (ΔΨM) at 40× magnification. In control cells, red JC-1 aggregates indicate intact mitochondrial membrane potential. In contrast, CS-(HMA-co-DEAEMA) treated cells displayed a higher intensity of green JC-1 monomers, reflecting loss of mitochondrial membrane potential.

b: Flow cytometry analysis of HT-29 cells treated with CS-(HMA-co-DEAEMA) for 24 h at 75, 125, and 175 μg/ml. A dose-dependent increase in pre-apoptotic cell populations was observed, with 22.42%, 68.93%, and 88.65% cells undergoing apoptosis compared to the control.

4. Conclusion

The present study successfully validates the proposed hypothesis that the rational incorporation of 2-hydroxyethyl methacrylate (HMA) and 2-(diethylamino)ethyl methacrylate (DEAEMA) into a chitosan-based hydrogel network can generate a multifunctional, pH-responsive, and mechanically stable biomaterial with selective anticancer activity. FTIR, 1H NMR, and XRD confirmed successful copolymer integration and reduced chitosan crystallinity, while SEM and BET analyses revealed porous, interconnected hydrogel networks. Rheological, TGA, and DSC analyses demonstrated improved mechanical integrity and thermal stability of the modified hydrogels. The pH-dependent swelling behaviour further confirmed the stimuli-responsive nature in acidic medium at 4,7 and 9 pH. Biological evaluation substantiated the second part of the hypothesis, demonstrating that the CS-(HMA-co-DEAEMA) hydrogel exhibits pronounced and selective cytotoxicity (IC50 value = 125.582 ± 9.118 μg/mL) toward HT-29 colorectal cancer cells while maintaining minimal toxicity toward normal HEK-293 cells. The observed antitumor efficacy was concentration-dependent and mediated through mitochondrial-associated apoptotic pathways, as evidenced by nuclear morphological changes and significant loss of mitochondrial membrane potential (7.28%). In contrast, single-monomer chitosan hydrogels showed comparatively lower anticancer activity, highlighting the synergistic effect of HMA and DEAEMA copolymerization.

Collectively, these findings confirm that the designed CS-(HMA-co-DEAEMA) hydrogel fulfils the intended structural, functional, and biological criteria, thereby validating the research hypothesis. The study establishes this hydrogel system as a promising, biocompatible, and intelligent platform for colorectal cancer-oriented biomedical and drug delivery applications. The present study systematically developed chitosan-based hydrogels with tunable physicochemical and rheological properties, supported by comprehensive structural, morphological, pH-responsive, and in-vitro anticancer evaluations. Cytotoxicity, DAPI staining, and mitochondrial membrane-potential analyses provided complementary insights into cellular responses; however, further validation using additional colorectal cancer and normal intestinal cell models, along with in-vivo studies, long-term stability/biodegradation assessments, and detailed molecular analyses, is needed to establish therapeutic applicability and elucidate the underlying mechanism.

CRediT authorship contribution statement

Ashlesha P. Kawale: Writing – original draft, Software, Methodology, Investigation, Data curation. Anand Patel: Writing – original draft, Software, Methodology, Data curation. Shiwani Singh: Investigation, Formal analysis, Data curation. Paramjeet Yadav: Investigation, Formal analysis, Data curation. Nishant Shekhar: Software, Formal analysis, Data curation. Arti Srivastava: Supervision, Resources, Methodology, Conceptualization. Arbind Acharya: Writing – review & editing, Validation, Supervision, Resources. Rajesh Kumar: Writing – review & editing, Validation, Supervision, Resources, Methodology, Investigation, Formal analysis. Neha Jain: Data curation.

Declaration of competing interest

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

Acknowledgements

The authors gratefully acknowledge the financial support provided by Banaras Hindu University under the IoE Scheme (No. 6031).

Data availability

All the experimental data is included as a supporting document

References

View Abstract

来源 查看原文

版权申明 本网站立足国家海洋药物和生物制品产业联盟,致力于打造海洋生物医药“产学研用”一站式、综合性资讯共享服务平台,促进我国海洋药物和功能制品“资源链、科技链、产业链、应用链”协同创新、深度融合发展。本文转载自原文来源。版权归原作者及原来出处所有,部分文章未能联系到原作者,在此深表歉意。如涉及版权问题,请留言联系我们协商处理(邮箱:czhang@tio.org.cn),侵权内容将即刻删除。

免责声明 本文仅代表作者个人观点,与本平台立场无关。本站不对内容真实性、完整性、时效性作保证,仅供参考,请读者自行核实。